1 Scope*
1.1 This specification
2 covers 39 grades of annealed titanium and titanium alloy forgings as follows:
1.1.1 Grade F-1—UNS R50250. Unalloyed titanium,
1.1.2 Grade F-2—UNS R50400. Unalloyed titanium,
1.1.2.1 Grade F-2H—UNS R50400. Unalloyed titanium (Grade 2 with 58 ksi (400 MPa) minimum UTS),
1.1.3 Grade F-3—UNS R50550. Unalloyed titanium,
1.1.4 Grade F-4—UNS R50700. Unalloyed titanium,
1.1.5 Grade F-5—UNS R56400. Titanium alloy (6 % aluminum, 4 % vanadium),
1.1.6 Grade F-6—UNS R54520. Titanium alloy (5 % aluminum, 2.5 % tin),
1.1.7 Grade F-7—UNS R52400. Unalloyed titanium plus 0.12 to 0.25 % palladium,
1.1.7.1 Grade F-7H—UNS R52400. Unalloyed titanium plus 0.12 to 0.25 % palladium (Grade 7 with 58 ksi (400 MPa) minimum UTS),
1.1.8 Grade F-9—UNS R56320. Titanium alloy (3 % aluminum, 2.5 % vanadium),
1.1.9 Grade F-11—UNS R52250. Unalloyed titanium plus 0.12 to 0.25 % palladium,
1.1.10 Grade F-12—UNS R53400. Titanium alloy (0.3 % molybdenum, 0.8 % nickel),
1.1.11 Grade F-13—UNS R53413. Titanium alloy (0.5 % nickel, 0.05 % ruthenium),
1.1.12 Grade F-14—UNS R53414. Titanium alloy (0.5 % nickel, 0.05 % ruthenium),
1.1.13 Grade F-15—UNS R53415. Titanium alloy (0.5 % nickel, 0.05 % ruthenium),
1.1.14 Grade F-16—UNS R52402. Unalloyed titanium plus 0.04 to 0.08 % palladium,
1.1.14.1 Grade F-16H—UNS R52402. Unalloyed titanium plus 0.04 to 0.08 % palladium (Grade 16 with 58 ksi (400 MPa) minimum UTS),
1.1.15 Grade F-17—UNS R52252. Unalloyed titanium plus 0.04 to 0.08 % palladium,
1.1.16 Grade F-18—UNS R56322. Titanium alloy (3 % aluminum, 2.5 % vanadium) plus 0.04 % to 0.08 % palladium,
1.1.17 Grade F-19—UNS R58640. Titanium alloy (3 % aluminum, 8 % vanadium, 6 % chromium, 4 % zirconium, 4 % molybdenum),
1.1.18 Grade F-20—UNS R58645. Titanium alloy (3 % aluminum, 8 % vanadium, 6 % chromium, 4 % zirconium, 4 % molybdenum) plus 0.04 to 0.08 % palladium,
1.1.19 Grade F-21—UNS R58210. Titanium alloy (3 % aluminum, 2.7 % niobium, 15 % molybdenum, 0.25 % silicon),
1.1.20 Grade F-23—UNS R56407. Titanium alloy (6 % aluminum, 4 % vanadium, extra low interstitials, ELI),
1.1.21 Grade F-24—UNS R56405. Titanium alloy (6 % aluminum, 4 % vanadium) plus 0.04 to 0.08 % palladium,
1.1.22 Grade F-25—UNS R56403. Titanium alloy (6 % aluminum, 4 % vanadium) plus 0.3 to 0.8 % nickel and 0.04 to 0.08 % palladium,
1.1.23 Grade F-26—UNS R52404. Unalloyed titanium plus 0.08 to 0.14 % ruthenium,
1.1.23.1 Grade F-26H—UNS R52404. Unalloyed titanium plus 0.08 to 0.14 % ruthenium (Grade 26 with 58 ksi (400 MPa) minimum UTS),
1.1.24 Grade F-27—UNS R52254. Unalloyed titanium plus 0.08 to 0.14 % ruthenium,
1.1.25 Grade F-28—UNS R56323. Titanium alloy (3 % aluminum, 2.5 % vanadium plus 0.08 to 0.14 % ruthenium),
1.1.26 Grade F-29—UNS R56404. Titanium alloy (6 % aluminum, 4 % vanadium, extra low interstitial, ELI plus 0.08 to 0.14 % ruthenium),
1.1.27 Grade F-30—UNS R53530. Titanium alloy (0.3 % cobalt, 0.05 % palladium),
1.1.28 Grade F-31—UNS R53532. Titanium alloy (0.3 % cobalt, 0.05 % palladium),
1.1.29 Grade F-32—UNS R55111. Titanium alloy (5 % aluminum, 1 % vanadium, 1 % tin, 1 % zirconium, 0.8 % molybdenum),
1.1.30 Grade F-33—UNS R53442. Titanium alloy (0.4 % nickel, 0.015 % palladium, 0.025 % ruthenium, 0.15 % chromium),
1 This specification is under the jurisdiction of ASTM Committee B10 on, Reactive and Refractory Metals and Alloys and is the direct responsibility of, ` Subcommittee B10.01 on Titanium.,,
Current edition approved July 1, 2013. Published August 2013. Originally,,, ` approved in 1961. Last previous edition approved in 2010 as B381 – 10
ε1
. DOI:-- 10.1520/B0381-13., ,
2 For ASME Boiler and Pressure Vessel Code applications, see related Specifi-, , cation SB-381 in Section II of that Code.---
1.1.31 Grade F-34—UNS R53445. Titanium alloy (0.4 % nickel, 0.015 % palladium, 0.025 % ruthenium, 0.15 % chromium),
1.1.32 Grade F-35—UNS R56340. Titanium alloy (4.5 % aluminum, 2 % molybdenum, 1.6 % vanadium, 0.5 % iron, 0.3 % silicon),
1.1.33 Grade F-36—UNS R58450. Titanium alloy (45 % niobium),
1.1.34 Grade F-37—UNS R52815. Titanium alloy (1.5 % aluminum), and
1.1.35 Grade F-38—UNS R54250. Titanium alloy (4 % aluminum, 2.5 % vanadium, 1.5 % iron). NOTE 1—H grade material is identical to the corresponding numeric grade (that is, Grade 2H = Grade 2) except for the higher guaranteed minimum UTS, and may always be certified as meeting the requirements of its corresponding numeric grade. Grades 2H, 7H, 16H, and 26H are intended primarily for pressure vessel use.
1.2 The values stated in inch-pound units are to be regarded as standard. The values given in parentheses are mathematical conversions to SI units that are provided for information only and are not considered standard.
2 Referenced Documents
2.1 ASTM Standards:
3
B348 Specification for Titanium and Titanium Alloy Bars and Billets E8 Test Methods for Tension Testing of Metallic Materials
E29 Practice for Using Significant Digits in Test Data to Determine Conformance with Specifications
E539 Test Method for Analysis of Titanium Alloys by X-Ray Fluorescence Spectrometry
E1409 Test Method for Determination of Oxygen and Nitrogen in Titanium and Titanium Alloys by the Inert Gas Fusion Technique
E1447 Test Method for Determination of Hydrogen in Titanium and Titanium Alloys by Inert Gas Fusion Thermal Conductivity/Infrared Detection Method
E1941 Test Method for Determination of Carbon in Refractory and Reactive Metals and Their Alloys by Combustion Analysis
E2371 Test Method for Analysis of Titanium and Titanium Alloys by Direct Current Plasma and Inductively Coupled Plasma Atomic Emission Spectrometry (Performance-Based Test Methodology)
E2626 Guide for Spectrometric Analysis of Reactive and Refractory Metals
3 Terminology
3.1 Definitions of Terms Specific to This Standard:
3.1.1 bar, n—a hot rolled, forged or cold worked semifinished solid section product whose cross sectional area is less than 16 in.
2 (10 323 mm
2
).
3.1.2 billet, n—a solid semifinished section, hot rolled or forged from an ingot, with a cross sectional area greater than 16 in.
2 (10 323 mm
2
).
3.1.3 forging, n—any product of work on metal formed to a desired shape by impact or pressure in hammers, forging machines, upsetters presses or related forming equipment.
4 Ordering Information
4.1 Orders for forgings under this specification shall include the following information, as applicable:
4.1.1 Grade number (Section 1),
4.1.2 Tensile properties (Table 1),
4.1.3 Dimensions and tolerances (Section 10),
4.1.4 Sampling, mechanical properties (Section 8),
4.1.5 Methods for chemical analysis (Section 6),
4.1.6 Marking (Section 17),
4.1.7 Packaging (Section 17),
4.1.8 Certification (Section 16),
4.1.9 Disposition of rejected material (Section 14), and
4.1.10 Supplementary requirements (S1).
5 Materials and Manufacture
5.1 Material conforming to the latest revision of Specification B348 shall be used when producing forgings to this specification.
6 Chemical Composition
6.1 The grades of titanium and titanium alloy metal covered by this specification shall conform to the requirements as to chemical composition prescribed in Table 2.
6.1.1 The elements listed in Table 2 are intentional alloy additions or elements which are inherent to the manufacturer of titanium sponge, ingot or mill product.
6.1.1.1 Elements other than those listed in Table 2 are deemed to be capable of occurring in the grades listed in Table 2 by and only by way of unregulated or unanalyzed scrap additions to the ingot melt. Therefore, product analysis for elements not listed in Table 2 shall not be required unless specified and shall be considered to be in excess of the intent of this specification.
6.1.2 Elements intentionally added to the melt must be identified, analyzed, and reported in the chemical analysis.
6.2 When agreed upon by the producer and purchaser and requested by the purchaser in his written purchase order, chemical analysis shall be completed for specific residual elements not listed in this specification.
6.3 Product Analysis—Product analysis tolerances do not broaden the specified heat analysis requirements, but cover variations between laboratories in the measurement of chemical content. The manufacturer shall not ship material which is outside the limits specified in Table 2 for the applicable grade. Product analysis limits shall be as specified in Table 3.
6.4 Sampling—Samples for chemical analysis shall be representative of material being tested. Except for hydrogen and unless otherwise specified, chemical analysis of ingot or billet shall be reported. Samples for hydrogen determination shall be obtained from the forgings on a test basis and a frequency as agreed upon between the forger and the purchaser. The utmost care must be used in sampling titanium for chemical analysis because of its great affinity for elements such as oxygen,
3 For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards volume information, refer to the standard’s Document Summary page on the ASTM website.
| Grade | Tensile Strength, min | Yield Strength (0.2 % Offset), min or Range | Elongation in 4D, min, % | Reduction of Area, min, % | ||
| ksi | (MPa) | ksi | (MPa) | |||
| F-1 | 35 | (240) | 20 | (138) | 24 | 30 |
| F-2 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-2HB,C | 58 | (400) | 40 | (275) | 20 | 30 |
| F-3 | 65 | (450) | 55 | (380) | 18 | 30 |
| F-4 | 80 | (550) | 70 | (483) | 15 | 25 |
| F-5 | 130 | (895) | 120 | (828) | 10 | 25 |
| F-6 | 120 | (828) | 115 | (795) | 10 | 25 |
| F-7 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-7HB,C | 58 | (400) | 40 | (275) | 20 | 30 |
| F-9 | 120 | (828) | 110 | (759) | 10 | 25 |
| F-9D | 90 | (620) | 70 | (483) | 15 | 25 |
| F-11 | 35 | (240) | 20 | (138) | 24 | 30 |
| F-12 | 70 | (483) | 50 | (345) | 18 | 25 |
| F-13 | 40 | (275) | 25 | (170) | 24 | 30 |
| F-14 | 60 | (410) | 40 | (275) | 20 | 30 |
| F-15 | 70 | (483) | 55 | (380) | 18 | 25 |
| F-16 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-16HB,C | 58 | (400) | 40 | (275) | 20 | 30 |
| F-17 | 35 | (240) | 20 | (138) | 24 | 30 |
| F-18 | 90 | (620) | 70 | (483) | 15 | 25 |
| F-18D | 90 | (620) | 70 | (483) | 12 | 20 |
| F-19E | 115 | (793) | 110 | (759) | 15 | 25 |
| F-19F | 135 | (930) | 130 to 159 | (897) to (1096) | 10 | 20 |
| F-19G | 165 | (1138) | 160 to 185 | (1104) to (1276) | 5 | 20 |
| F-20E | 115 | (793) | 110 | (759) | 15 | 25 |
| F-20F | 135 | (930) | 130 to 159 | (897) to (1096) | 10 | 20 |
| F-20G | 165 | (1138) | 160 to 185 | (1104) to (1276) | 5 | 20 |
| F-21E | 115 | (793) | 110 | (759) | 15 | 35 |
| F-21F | 140 | (966) | 130 to 159 | (897) to (1096) | 10 | 30 |
| F-21G | 170 | (1172) | 160 to 185 | (1104) to (1276) | 8 | 20 |
| F-23 | 120 | (828) | 110 | (759) | 10 | 25 |
| F-23D | 120 | (828) | 110 | (759) | 7.5H, 6.0I | 25 |
| F-24 | 130 | (895) | 120 | (828) | 10 | 25 |
| F-25 | 130 | (895) | 120 | (828) | 10 | 25 |
| F-26 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-26HB,C | 58 | (400) | 40 | (275) | 20 | 30 |
| F-27 | 35 | (240) | 20 | (138) | 24 | 30 |
| F-28 | 90 | (620) | 70 | (483) | 15 | 25 |
| F-28D | 90 | (620) | 70 | (483) | 12 | 20 |
| F-29 | 120 | (828) | 110 | (759) | 10 | 25 |
| F-29D | 120 | (828) | 110 | (759) | 7.5H, 6.0I | 15 |
| F-30 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-31 | 65 | (450) | 55 | (380) | 18 | 30 |
| F-32 | 100 | (689) | 85 | (586) | 10 | 25 |
| F-33 | 50 | (345) | 40 | (275) | 20 | 30 |
| F-34 | 65 | (450) | 55 | (380) | 18 | 30 |
| F-35 | 130 | (895) | 120 | (828) | 5 | 20 |
| F-36 | 65 | (450) | 60 to 95 | (410 to 655) | 10 | ... |
| F-37 | 50 | (345) | 31 | (215) | 20 | 30 |
| F-38 | 130 | (895) | 115 | (794) | 10 | 25 |
nitrogen, and hydrogen. Therefore, the cutting and handling of samples should include practices that will prevent contamination. Samples shall be collected from clean metal.
6.5 At least two samples for chemical analysis shall be tested to determine chemical composition. Samples shall be taken from opposite extremes of the product to be analyzed.
| Grade | UNS Number | Carbon, max. | Oxygen range or max. | Nitrogen, Hydrogen, max. | Iron range or max. | Composition, Weight PercentA,B,C,D,E | Other Elements,Elements, max. each | Other total | ||||||||||||
| Aluminum | Vanadium | Palladium | Ruthenium | Nickel | Molybdenum | Chromium | Cobalt | Zirconium | Niobium | Tin | Silicon | |||||||||
| F-1 | R50250 | 0.08 | 0.18 | 0.03 | 0.015 | 0.20 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-2/ F-2H | R50400 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-3 | R50550 | 0.08 | 0.35 | 0.05 | 0.015 | 0.30 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-4 | R50700 | 0.08 | 0.40 | 0.05 | 0.015 | 0.50 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-5 | R56400 | 0.08 | 0.20 | 0.05 | 0.015 | 0.40 | 5.5-6.75 | 3.5-4.5 | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-6 | R54520 | 0.08 | 0.20 | 0.03 | 0.015 | 0.50 | 4.0-6.0 | -- | -- | -- | -- | -- | -- | -- | -- | -- | 2.0-3.0 | -- | 0.1 | 0.4 |
| F-7/ F-7H | R52400 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | 0.12-0.25 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-9 | R56320 | 0.08 | 0.15 | 0.03 | 0.015 | 0.25 | 2.5-3.5 | 2.0-3.0 | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-11 | R52250 | 0.08 | 0.18 | 0.03 | 0.015 | 0.20 | -- | -- | 0.12-0.25 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-12 | R53400 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | -- | -- | 0.6-0.9 | 0.2-0.4 | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-13 | R53413 | 0.08 | 0.10 | 0.03 | 0.015 | 0.20 | -- | -- | -- | 0.04-0.06 | 0.4-0.6 | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-14 | R53414 | 0.08 | 0.15 | 0.03 | 0.015 | 0.30 | -- | -- | -- | 0.04-0.06 | 0.4-0.6 | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-15 | R53415 | 0.08 | 0.25 | 0.05 | 0.015 | 0.30 | -- | -- | -- | 0.04-0.06 | 0.4-0.6 | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-16/ F-16H | R52402 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | 0.04-0.08 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-17 | R52252 | 0.08 | 0.18 | 0.03 | 0.015 | 0.20 | -- | -- | 0.04-0.08 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-18 | R56322 | 0.08 | 0.15 | 0.03 | 0.015 | 0.25 | 2.5-3.5 | 2.0-3.0 | 0.04-0.08 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-19 | R58640 | 0.05 | 0.12 | 0.03 | 0.02 | 0.30 | 3.0-4.0 | 7.5-8.5 | -- | -- | -- | 3.5-4.5 | 5.5-6.5 | -- | 3.5-4.5 | -- | -- | 0.15 | 0.4 | |
| F-20 | R58645 | 0.05 | 0.12 | 0.03 | 0.02 | 0.30 | 3.0-4.0 | 7.5-8.5 | 0.04-0.08 | -- | -- | 3.5-4.5 | 5.5-6.5 | -- | 3.5-4.5 | -- | -- | 0.15 | 0.4 | |
| F-21 | R58210 | 0.05 | 0.17 | 0.03 | 0.015 | 0.40 | 2.5-3.5 | -- | -- | -- | -- | 14.0-16.0 | -- | -- | -- | 2.2-3.2 | -- | 0.15-0.25 | 0.1 | |
| F-23 | R56407 | 0.08 | 0.13 | 0.03 | 0.0125 | 0.25 | 5.5-6.5 | 3.5-4.5 | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-24 | R56405 | 0.08 | 0.20 | 0.05 | 0.015 | 0.40 | 5.5-6.75 | 3.5-4.5 | 0.04-0.08 | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-25 | R56403 | 0.08 | 0.20 | 0.05 | 0.015 | 0.40 | 5.5-6.75 | 3.5-4.5 | 0.04-0.08 | -- | 0.3-0.8 | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-26/ F-16H | R52404 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | -- | 0.08-0.14 | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-27 | R52254 | 0.08 | 0.18 | 0.03 | 0.015 | 0.20 | -- | -- | -- | 0.08-0.14 | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-28 | R56323 | 0.08 | 0.15 | 0.03 | 0.015 | 0.25 | 2.5-3.5 | 2.0-3.0 | -- | 0.08-0.14 | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-29 | R56404 | 0.08 | 0.13 | 0.03 | 0.0125 | 0.25 | 5.5-6.5 | 3.5-4.5 | -- | 0.08-0.14 | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 | |
| F-30 | R53530 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | 0.04-0.08 | -- | -- | -- | -- | 0.20-0.80 | -- | -- | -- | 0.1 | 0.4 | |
| F-31 | R53532 | 0.08 | 0.35 | 0.05 | 0.015 | 0.30 | -- | -- | 0.04-0.08 | -- | -- | -- | -- | 0.20-0.80 | -- | -- | -- | 0.1 | 0.4 | |
B381 - 13
| Grade | UNS Number | Carbon, max. | Oxygen range or max. | Nitrogen, max. | Hydrogen, max. | Iron range or max. | Aluminum | Vanadium | Palladium | Ruthenium | Nickel | Molybdenum | Chromium | Cobalt | Zirconium | Niobium | Tin | Silicon | Other Elements, max. each | Other Elements, max. total |
| F-32 | R55111 | 0.08 | 0.11 | 0.03 | 0.015 | 0.25 | 4.5-5.5 | 0.6-1.4 | -- | -- | -- | 0.6-1.2 | -- | -- | 0.6-1.4 | -- | 0.6-1.4 | 0.06-0.14 | 0.1 | 0.4 |
| F-33 | R53442 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | -- | -- | 0.01-0.02 | 0.02-0.04 | 0.35-0.55 | -- | 0.1-0.2 | -- | -- | -- | -- | -- | 0.1 | 0.4 |
| F-34 | R53445 | 0.08 | 0.35 | 0.05 | 0.015 | 0.30 | -- | -- | 0.01-0.02 | 0.02-0.04 | 0.35-0.55 | -- | 0.1-0.2 | -- | -- | -- | -- | -- | 0.1 | 0.4 |
| F-35 | R56340 | 0.08 | 0.25 | 0.05 | 0.015 | 0.20-0.80 | 4.0-5.0 | 1.1-2.1 | -- | -- | -- | 1.5-2.5 | -- | -- | -- | -- | -- | 0.20-0.40 | 0.1 | 0.4 |
| F-36 | R58450 | 0.04 | 0.16 | 0.03 | 0.015 | 0.03 | -- | -- | -- | -- | -- | -- | -- | -- | -- | 42.0-47.0 | -- | -- | 0.1 | 0.4 |
| F-37 | R52815 | 0.08 | 0.25 | 0.03 | 0.015 | 0.30 | 1.0-2.0 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 |
| F-38 | R54250 | 0.08 | 0.20-0.30 | 0.03 | 0.015 | 1.2-1.8 | 3.5-4.5 | 2.0-3.0 | -- | -- | -- | -- | -- | -- | -- | -- | -- | -- | 0.1 | 0.4 |
B381 - 13
| Product Analysis | Permissible | |
| Element | Limits, max or Range, % | Variation in Product Analysis |
| Aluminum | 0.5 to 2.5 | ±0.20 |
| Aluminum | 2.5 to 6.75 | ±0.40 |
| Carbon | 0.10 | +0.02 |
| Chromium | 0.1 to 0.2 | ±0.02 |
| Chromium | 5.5 to 6.5 | ±0.30 |
| Cobalt | 0.2 to 0.8 | ±0.05 |
| Hydrogen | 0.02 | +0.002 |
| Iron | 0.80 | +0.15 |
| Iron | 1.2 to 1.8 | ±0.20 |
| Molybdenum | 0.2 to 0.4 | ±0.03 |
| Molybdenum | 0.6 to 1.2 | ±0.15 |
| Molybdenum | 1.5 to 4.5 | ±0.20 |
| Molybdenum | 14.0 to 16.0 | ±0.50 |
| Nickel | 0.3 to 0.9 | ±0.05 |
| Niobium | 2.2 to 3.2 | ±0.15 |
| Niobium | >30 | ±0.50 |
| Nitrogen | 0.05 | +0.02 |
| Oxygen | 0.30 | +0.03 |
| Oxygen | 0.31 to 0.40 | ±0.04 |
| Palladium | 0.01 to 0.02 | ±0.002 |
| Palladium | 0.04 to 0.08 | ±0.005 |
| Palladium | 0.12 to 0.25 | ±0.02 |
| Ruthenium | 0.02 to 0.04 | ±0.005 |
| Ruthenium | 0.04 to 0.06 | ±0.005 |
| Ruthenium | 0.08 to 0.14 | ±0.01 |
| Silicon | 0.06 to 0.40 | ±0.02 |
| Tin | 0.6 to 3.0 | ±0.15 |
| Vanadium | 0.6 to 4.5 | ±0.15 |
| Vanadium | 7.5 to 8.5 | ±0.40 |
| Zirconium | 0.6 to 1.4 | ±0.15 |
| Zirconium | 3.5 to 4.5 | ±0.20 |
| ResidualsA (each) | 0.15 | +0.02 |
7 Methods of Chemical Analysis
7.1 The chemical analysis shall normally be conducted using the ASTM standard test methods referenced in 2.1. Other industry standard methods may be used where the ASTM test methods in 2.1 do not adequately cover the elements in the material or by agreement between the producer and purchaser. Alternate techniques are discussed in Guide E2626.
8 Mechanical Properties
8.1 Forgings supplied under this specification shall conform to the requirements as to mechanical properties specified in Table 1, as applicable.
8.2 Specimens for tension tests shall be machined and tested in accordance with Test Methods E8. Tensile properties shall be determined using a strain rate of 0.003 to 0.007 in./in.·min through the specified yield strength. After the specified yield strength has been reached, the crosshead speed shall be increased to a rate sufficient to produce fracture in approximately one additional minute.
8.3 Sampling—Tension test specimens shall be machined from material as agreed upon by the manufacturer and the purchaser.
9 Nondestructive Tests
9.1 Nondestructive test requirements such as ultrasonic test, X ray, or surface inspection shall be specified by the purchaser, if required. The standard for acceptance or rejection shall be agreed upon between the forger and the purchaser.
10 Dimensions and Permissible Variations
10.1 Dimensions and tolerances of titanium and titanium alloy forgings covered by this specification shall be as shown on the applicable forging drawing or otherwise agreed upon by the manufacturer and the purchaser.
11 Workmanship, Finish, and Appearance
11.1 Titanium alloy forgings shall be free of injurious external and internal imperfections of a nature that will interfere with the purpose for which they are intended. Annealed forgings may be furnished as descaled, sandblasted, or ground. The manufacturer shall be permitted to remove minor surface imperfections by spot grinding if such grinding does not reduce the thickness of the forging below the minimum permitted by the tolerance for the forging at the applicable location.
12 Retests
12.1 If the results of any chemical or mechanical property test lot are not in conformance with the requirements of this specification, the lot may be retested at the option of the manufacturer. The frequency of the retest will double the initial number of tests. If the results of the retest conform to the specification, then the retest values will become the test values for certification. Only original conforming test results or the conforming retest results shall be reported to the purchaser. If the results for the retest fail to conform to the specification, the material will be rejected in accordance with Section 14.
13 Rounding-Off Procedure
13.1 For purposes of determining conformance with this specification, an observed or a calculated value shall be rounded off to the nearest“ unit” in the last right-hand significant digit used in expressing the limiting value. This is in accordance with the round-off method of Practice E29.
14 Rejection
14.1 Forgings not conforming to this specification or to authorized modifications shall be subject to rejection. Unless otherwise specified, rejected forgings may be returned to the manufacturer at the manufacturer’s expense, unless the purchaser receives, within three weeks of notice of rejection, other instructions for disposition.
15 Referee Test and Analysis
15.1 In the event of disagreement between the manufacturer and the purchaser on the conformance of the material to the requirements of this specification, a mutually acceptable referee shall perform the tests in question using the ASTM standard methods in 2.1. The referee’s testing shall be used in determining conformance of the material to this specification.
16 Certification
16.1 The manufacturer shall supply at least one copy of the report certifying that the material supplied has been manufactured, inspected, sampled, and tested in accordance with the requirements of this specification and that the results of chemical analysis, tensile, and other tests meet the requirements of the specification for the grade specified. The report shall include results of all chemical analysis, tensile tests, and all other tests required by the specification.
17 Packaging and Package Marking
17.1 Packaging—Unless otherwise specified, forgings purchased under this specification shall be packaged in accordance with the manufacturer’s standard practice.
17.2 Marking—Forgings shall be marked for identification as agreed upon by the manufacturer and the purchaser.
18 Keywords
18.1 forgings; titanium; titanium alloys
SUPPLEMENTARY REQUIREMENTS
SUPPLEMENTARY REQUIREMENTS COVERING GRADE F3 TITANIUM FORGINGS
The following supplementary requirements are primarily intended for U.S. military applications and shall apply only when specified by the purchaser in the inquiry, contract, or order.
S1. U.S. Military Requirements
S1.1 Referenced Documents section follows.
S1.2 Unless otherwise specified in the contract or purchase order, the seller is responsible for the performance of all inspection and test requirements in this specification, and the seller may use his or other suitable facilities for the perfor--- mance of the inspection and testing., ``,
S1.3 Grade F-3 composition shall be modified as follows:`,, Hydrogen,,,, 0.0125 max Iroǹ,, 0.20 max Oxygen``- 0.26 max
S1.4 Two tensile specimens shall be taken from each lot of,, ,, forgings up to and 125 pounds, and two tensile specimens shall,,` be taken from each forging greater than 125 pounds for verification of compliance with Grade F-3 mechanical properties of Table 3. A lot shall constitute all forgings from the same heat, of the same design and size and heat treated in the same heat treat furnace load. The test specimens shall be taken from integral prolongations or extra forgings may be provided by the forger. Forgings under 3
1
⁄2 in. (90 mm) in cross section may use separately forged test bars provided the wall thickness and amount of working are equivalent to the forgings being supplied. Extra forgings may be provided for samples when forgings are over 3
1
⁄2 in. (90 mm) in cross section provided samples cannot be taken from prolongations or by trepanning. Samples shall be taken from the section of forging having the largest cross section. The longitudinal axis of the tensile specimens shall be parallel to the major direction of metal flow in the forging.
S1.5 Repair welding is not permitted.
S1.6 Each forging shall be ultrasonically inspected in accordance with MIL-STD-2154 throughout 100 % of their volume. Inspection shall be performed after heat treating when the forging is machined to the configuration for ultrasonic inspection as shown on the forging sketch or drawing. Inspection shall be performed prior to drilling holes, cutting keyways, tapers, grooves, or machining section to final contour. Forgings
shall be scanned using a straight beam technique such that all major planes are covered. Disc type forgings shall be scanned using a straight beam from at least one flat face and radially from the circumference when possible. Cylindrical, ring, and hollow forgings shall be scanned from the entire external surface using the straight beam technique, and in the axial direction to the maximum extent possible. Acceptance criteria shall be to class A of MIL-STD-2154.
S1.7 All surfaces of each forging shall be liquid penetrant inspected in accordance with NAVSEA T9074-AS-GIB-010/ 271. Acceptance criteria shall be in accordance with NAVSEA S9074-AR-GIB-010/278 as specified in the order.
S1.8 Forgings shall be free of foreign material and contaminants such as sulfur, lead, marking paints or machining or forming lubricants. Forgings shall be cleaned prior to any heat treatment operations. Forgings shall be free of any oxygen rich layer, such as alpha case.
S1.9 The first forging of each type and design submitted for inspection shall be the first article sample. Mechanical properties for first article inspections shall be determined throughout the forging as specified in the order (which should also include specific instructions regarding arrangements for examinations, approval of test results, and disposition of the first article samples), and the number and location of the test specimens and the acceptance criteria shall be as specified or as agreed upon between the contracting activity and the manufacturer. In addition, A full cross-section shall be macroetched in accordance with ASTM E340 and examined at 10× magnification for uniformity, soundness, grain size and grain flow. The macro etch cross section shall evidence uniformity of quality, soundness and freedom from cracks and porosity. A fully wrought structure shall be evident and variation in grain size shall be such that it will not interfere with ultrasonic examination. The manufacturer shall maintain a record of production practices used for the first article forging. In the event of change in the production practice in the same or subsequent
order, the manufacturer shall notify the contracting activity and obtain approval of the changes. The manufacturer may be required to perform specific first article tests and examinations to verify that the change will not or has not degraded forging quality.
S1.10 The material shall be electron beam and/or plasma melted or shall be multiple melted with at least one of the melting cycles under vacuum.
S2. Referenced Documents
S2.1 ASTM Standard:
E340 Test Method for Macroetching Metals and Alloys
S2.2 Military Standards:
T9074–AS-GIB-010/271 Requirements for Nondestructive Testing Methods
S9074–AR-GIB-010/278 Requirements for Fabrication Weldingand Inspection, and Casting Inspection and Repair for Machinery, Piping, and Pressure Vessels MIL-STD-2154 Inspection, Ultrasonic, Wrought Metals, Processing for
SUMMARY OF CHANGES
Committee B10 has identified the location of selected changes to this standard since the last issue (B381-10
ε1
) that may impact the use of this standard. (Approved July 1, 2013.)
(1) Added UNS Numbers under Scope and in Table 1. (2) Included metric equivalent UTS for H Grades in Scope. (3) Combined H Grade and standard numeric grade on one line in Table 1.
(4) Deleted note describing the historical rationale for the H Grades from Scope.
This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years and if not revised, either reapproved or withdrawn. Your comments are invited either for revision of this standard or for additional standards and should be addressed to ASTM International Headquarters. Your comments will receive careful consideration at a meeting of the responsible technical committee, which you may attend. If you feel that your comments have not received a fair hearing you should make your views known to the ASTM Committee on Standards, at the address shown below.

评论