1 Scope*
1.1 This specification
2 covers forged low alloy and stainless steel piping components for use in pressure systems. Included are flanges, fittings, valves, and similar parts to specified dimensions or to dimensional standards, such as the ASME specifications that are referenced in Section 2.
1.2 For bars and products machined directly from bar (other than those directly addressed by this specification; see 6.4), refer to Specifications A479/A479M and A739 for the similar grades available in those specifications. Products made to this specification are limited to a maximum weight of 10 000 lb [4540 kg]. For larger products and products for other applications, refer to Specifications A336/A336M and A965/A965M for the similar ferritic and austenitic grades, respectively, available in those specifications.
1.3 Several grades of low alloy steels and ferritic, martensitic, austenitic, and ferritic-austenitic stainless steels are included in this specification. Selection will depend upon design and service requirements. Several of the ferritic/austenitic (duplex) grades are also found in Specification A1049/ A1049M.
1.4 Supplementary requirements are provided for use when additional testing or inspection is desired. These shall apply only when specified individually by the purchaser in the order.
1.5 This specification is expressed in both inch-pound units and in SI units. However, unless the order specifies the applicable “M” specification designation (SI units), the material shall be furnished to inch-pound units.
1.6 The values stated in either SI units or inch-pound units are to be regarded separately as the standard. Within the text, the SI units are shown in brackets. The values stated in each
system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in non-conformance with the standard.
2 Referenced Documents
2.1 In addition to the referenced documents listed in Specification A961/A961M, the following list of standards apply to this specification.
2.2 ASTM Standards:
3
A262 Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels
A275/A275M Practice for Magnetic Particle Examination of Steel Forgings
A336/A336M Specification for Alloy Steel Forgings for Pressure and High-Temperature Parts
A370 Test Methods and Definitions for Mechanical Testing of Steel Products
A388/A388M Practice for Ultrasonic Examination of Steel Forgings
A479/A479M Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels
A484/A484M Specification for General Requirements for Stainless Steel Bars, Billets, and Forgings
A739 Specification for Steel Bars, Alloy, Hot-Wrought, for Elevated Temperature or Pressure-Containing Parts, or Both
A763 Practices for Detecting Susceptibility to Intergranular Attack in Ferritic Stainless Steels
A788/A788M Specification for Steel Forgings, General Requirements
A961/A961M Specification for Common Requirements for Steel Flanges, Forged Fittings, Valves, and Parts for Piping Applications
A965/A965M Specification for Steel Forgings, Austenitic, for Pressure and High Temperature Parts
1 This specification is under the jurisdiction of ASTM Committee A01 on Steel, Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee A01.22 on Steel Forgings and Wrought Fittings for Piping Applications and Bolting Materials for Piping and Special Purpose Applications.
Current edition approved June 1, 2011. Published June 2011. Originally approved in 1935. Last previous edition approved in 2010 as A182/A182M–10a. DOI: 10.1520/A0182_A0182M-11.
2 For ASME Boiler and Pressure Vessel Code applications see related Specification SA-182 in Section II of that Code.
3 For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards volume information, refer to the standard’s Document Summary page on the ASTM website.
A1049/A1049M Specification for Stainless Steel Forgings, Ferritic/Austenitic (Duplex), for Pressure Vessels and Related Components
E92 Test Method for Vickers Hardness of Metallic Materials
4
E112 Test Methods for Determining Average Grain Size
E165 Practice for Liquid Penetrant Examination for General Industry
E340 Test Method for Macroetching Metals and Alloys
2.3 ASME Boiler and Pressure Vessel Codes:
5
Section IX Welding and Brazing Qualifications
2.4 AWS Specifications
6
A5.4/A5.4M Specification for Stainless Steel Electrodes for Shielded Metal Arc Welding
A5.5/A5.5M Specification for Low-Alloy Steel Electrodes for Shielded Metal Arc Welding
A5.9/A5.9M Specification for Bare Stainless Steel Welding Electrodes and Rods
A5.11/A5.11M Specification for Nickel and Nickel-Alloy Welding Electrodes for Shielded Metal Arc Welding
A5.14/A5.14M Specification for Nickel and Nickel-Alloy Bare Welding Electrodes and Rods
A5.23/A5.23M Specification for Low-Alloy Steel Electrodes and Fluxes for Submerged Arc Welding
A5.28/A5.28M Specification for Low-Alloy Steel Electrodes for Gas Shielded Arc Welding
A5.29/A5.29M Low-Alloy Steel Electrodes for Flux Cored Arc Welding
3 Terminology
3.1 Definitions—For definitions of terms used in this specification, refer to Specification A961/A961M.
3.2 Definitions of Terms Specific to This Standard:
3.2.1 hardened condition, n—for F23, the metallurgical condition achieved after normalizing and cooling to room temperature but prior to tempering.
4 Ordering Information
4.1 It is the purchaser’s responsibility to specify in the purchase order information necessary to purchase the needed material. In addition to the ordering information guidelines in Specification A961/A961M, orders should include the following information:
4.1.1 Additional requirements (see 7.2.1, Table 2 footnotes, 9.3, and 19.2), and
4.1.2 Requirement, if any, that manufacturer shall submit drawings for approval showing the shape of the rough forging before machining and the exact location of test specimen material (see 9.3.1).
5 General Requirements
5.1 Product furnished to this specification shall conform to the requirements of Specification A961/A961M, including any supplementary requirements that are indicated in the purchase order. Failure to comply with the general requirements of Specification A961/A961M constitutes nonconformance with this specification. In case of conflict between the requirements of this specification and Specification A961/A961M, this specification shall prevail.
6 Manufacture
6.1 The low-alloy ferritic steels shall be made by the open-hearth, electric-furnace, or basic-oxygen process with the option of separate degassing and refining processes in each case.
6.2 The stainless steels shall be melted by one of the following processes: (a) electric-furnace (with the option of separate degassing and refining processes); (b) vacuumfurnace; or (c) one of the former followed by vacuum or electroslag-consumable remelting. Grade F XM-27Cb may be produced by electron-beam melting.
6.3 A sufficient discard shall be made to secure freedom from injurious piping and undue segregation.
6.4 The material shall be forged as close as practicable to the specified shape and size.
6.4.1 Flanges of any type, elbows, return bends, tees, and header tees shall not be machined directly from bar stock.
6.4.2 Cylindrically-shaped parts may be machined from forged or rolled solution-annealed austenitic stainless steel bar without additional hot working.
6.4.3 Small cylindrically-shaped low alloy and martensitic stainless steel parts, NPS-4 [DN 100] and under, may be machined from forged or rolled bar, without additional hot working.
6.5 Except as provided for in 6.4, the finished product shall be a forging as defined in the Terminology section of Specification A788/A788M.
7 Heat Treatment 7
7.1 After hot working, forgings shall be cooled to a temperature below 1000 °F [538 °C] prior to heat treating in accordance with the requirements of Table 1.
7.2 Low Alloy Steels and Ferritic and Martensitic Stainless Steels—The low alloy steels and ferritic and martensitic stainless steels shall be heat treated in accordance with the requirements of 7.1 and Table 1. When more than one heat treatment option is listed for a Grade in Table 1, any one of the heat treatments listed shall be performed. The selection of the heat treatment shall be at the manufacturer’s option, unless otherwise stated in the purchase order.
7.2.1 Liquid Quenching—Except as permitted in 7.2.2, for F 1, F 2, and F 3, and in 7.2.3, for F 91, and when agreed to by
4 Withdrawn. The last approved version of this historical standard is referenced on www.astm.org.
5 Available from American Society of Mechanical Engineers (ASME), ASME International Headquarters, Three Park Ave., New York, NY 10016-5990, http:// www.asme.org.
6 Available from American Welding Society (AWS), 550 NW LeJeune Rd., Miami, FL 33126, http://www.aws.org.
7 A solution annealing temperature above 1950 °F [1065 °C] may impair the resistance to intergranular corrosion after subsequent exposure to sensitizing conditions in F 321, F 321H, F 347, F 347H, F 348, and F 348H. When specified by the purchaser, a lower temperature stabilization or resolution annealing shall be used subsequent to the initial high temperature solution anneal (see Supplementary Requirement S10).
the purchaser, liquid quenching followed by tempering shall be permitted provided the temperatures in Table 1 for each grade are used.
7.2.1.1 Marking—Parts that are liquid quenched and tempered shall be marked “QT.”
7.2.2 Alternatively, Grade F 1, F 2, and F 12, Classes 1 and 2 may be given a heat treatment of 1200 °F [650 °C] minimum after final hot or cold forming.
7.2.3 Alternatively, Grade F 91 forged fittings having any section thickness greater than 3 in. [75 mm], at the time of heat treatment, shall be normalized and tempered or quenched and tempered at the manufacturer’s option, provided that the temperatures in Table 1 for F 91 are used.
7.3 Austenitic and Ferritic-Austenitic Stainless Steels—The austenitic and ferritic-austenitic stainless steels shall be heat treated in accordance with the requirements of 7.1 and Table 1.
7.3.1 Alternatively, immediately following hot working, while the temperature of the forging is not less than the
minimum solution annealing temperature specified in Table 1, forgings made from austenitic grades (except grades F 304H, F 309H, F 310, F 310H, F 316H, F 321, F 321H, F 347, F 347H, F 348, F 348H, F 45, and F 56) may be individually rapidly quenched in accordance with the requirements of Table 1.
7.3.2 See Supplementary Requirement S8 if a particular heat treatment method is to be employed.
7.4 Time of Heat Treatment—Heat treatment of forgings may be performed before machining.
7.5 Forged or Rolled Bar—Forged or rolled austenitic stainless bar from which cylindrically shaped parts are to be machined, as permitted by 6.4, and the parts machined from such bar, without heat treatment after machining, shall be furnished to the annealing requirements of Specification A479/ A479M or this specification, with subsequent light cold drawing and straightening permitted (see Supplementary Requirement S3 if annealing must be the final operation).
| Grade | Heat Treat Type | Austenitizing/Solutioning Temperature, Minimum or Range, °F [°C]A | Cooling Media | Quenching Cool Below °F [°C] | Tempering Temperature, Minimum or Range, °F [°C] |
| Low Alloy Steels | |||||
| F 1 | anneal | 1650 [900] | furnace cool | B | B |
| normalize and temper | 1650 [900] | air cool | B | 1150 [620] | |
| F 2 | anneal | 1650 [900] | furnace cool | B | B |
| normalize and temper | 1650 [900] | air cool | B | 1150 [620] | |
| F 5, F 5a | anneal | 1750 [955] | furnace cool | B | B |
| normalize and temper | 1750 [955] | air cool | B | 1250 [675] | |
| F 9 | anneal | 1750 [955] | furnace cool | B | B |
| normalize and temper | 1750 [955] | air cool | B | 1250 [675] | |
| F 10 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 91 | normalize and temper | 1900-1975 [1040-1080] | air cool | B | 1350-1470 [730-800] |
| F 92 | normalize and temper | 1900-1975 [1040-1080] | air cool | B | 1350-1470 [730-800] |
| F 122 | normalize and temper | 1900-1975 [1040-1080] | air cool | B | 1350-1470 [730-800] |
| F 911 | normalize and temper | 1900-1975 [1040-1080] | air cool or liquid | B | 1365-1435 [740-780] |
| F 11, Class 1, 2, 3 | anneal | 1650 [900] | furnace cool | B | B |
| normalize and temper | 1650 [900] | air cool | B | 1150 [620] | |
| F 12, Class 1, 2 | anneal | 1650 [900] | furnace cool | B | B |
| normalize and temper | 1650 [900] | air cool | B | 1150 [620] | |
| F 21, F 3V, and F 3VCb | anneal | 1750 [955] | furnace cool | B | B |
| normalize and temper | 1750 [955] | air cool | B | 1250 [675] | |
| F 22, Class 1, 3 | anneal | 1650 [900] | furnace cool | B | B |
| normalize and temper | 1650 [900] | air cool | B | 1250 [675] | |
| F 22V | normalize and temper or quench and temper | 1650 [900] | air cool or liquid | B | 1250 [675] |
| F 23 | normalize and temper | 1900-1975 [1040-1080] | air cool accelerated cool | B | 1350-1470 [730-800] |
| F 24 | normalize and temper | 1800-1975 [980-1080] | air cool or liquid | B | 1350-1470 [730-800] |
| FR | anneal | 1750 [955] | furnace cool | B | B |
| normalize | 1750 [955] | air cool | B | B | |
| normalize and temper | 1750 [955] | air cool | B | 1250 [675] | |
| F 36, Class 1 | normalize and temper | 1650 [900] | air cool | B | 1100 [595] |
| F 36, Class 2 | normalize and temper | 1650 [900] | air cool | B | 1100 [595] |
| quench and temper | 1650 [900] | accelerated air cool or liquid | 1100 [595] | ||
| Martensitic Stainless Steels | |||||
| F 6a Class 1 | anneal | not specified | furnace cool | B | B |
| normalize and temper | not specified | air cool | 400 [205] | 1325 [725] | |
| temper | not required | B | B | 1325 [725] | |
| F 6a Class 2 | anneal | not specified | furnace cool | B | B |
| normalize and temper | not specified | air cool | 400 [205] | 1250 [675] | |
| temper | not required | B | B | 1250 [675] | |
| F 6a Class 3 | anneal | not specified | furnace cool | B | B |
| normalize and temper | not specified | air cool | 400 [205] | 1100 [595] | |
| Grade | Heat Treat Type | Austenitizing/Solutioning Temperature, Minimum or Range, °F [°C]A | Cooling Media | Quenching Cool Below °F [°C] | Tempering Temperature, Minimum or Range, °F [°C] |
| F 6a Class 4 | anneal | not specified | furnace cool | B | B |
| normalize and temper | not specified | air cool | 400 [205] | 1000 [540] | |
| F 6b | anneal | 1750 [955] | furnace cool | B | B |
| normalize and temper | 1750 [955] | air cool | 400 [205] | 1150 [620] | |
| F 6NM | normalize and temper | 1850 [1010] | air cool | 200 [95] | 1040-1120 [560-600] |
| Ferritic Stainless Steels | |||||
| F XM-27 Cb | anneal | 1850 [1010] | furnace cool | B | B |
| F 429 | anneal | 1850 [1010] | furnace cool | B | B |
| F 430 | anneal | not specified | furnace cool | B | B |
| Austenitic Stainless Steels | |||||
| F 304 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 304H | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 304L | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 304N | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 304LN | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 309H | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 310 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 310H | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 310MoLN | solution treat and quench | 1900-2010 [1050-1100] | liquid | 500 [260] | B |
| F 316 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 316H | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 316L | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 316N | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 316LN | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 316Ti | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 317 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 317L | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| S31727 | solution treat and quench | 1975-2155 [1080-1180] | liquid | 500 [260] | B |
| S32053 | solution treat and quench | 1975-2155 [1080-1180] | liquid | 500 [260] | B |
| F 347 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 347H | solution treat and quench | 2000 [1095] | liquid | 500 [260] | B |
| F 347LN | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 348 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 348H | solution treat and quench | 2000 [1095] | liquid | 500 [260] | B |
| F 321 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 321H | solution treat and quench | 2000 [1095] | liquid | 500 [260] | B |
| F XM-11 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F XM-19 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 20 | solution treat and quench | 1700-1850 [925-1010] | liquid | 500 [260] | B |
| F 44 | solution treat and quench | 2100 [1150] | liquid | 500 [260] | B |
| F 45 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 46 | solution treat and quench | 2010-2140 [1100-1140] | liquid | 500 [260] | B |
| F 47 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 48 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 49 | solution treat and quench | 2050 [1120] | liquid | 500 [260] | B |
| F 56 | solution treat and quench | 2050-2160 [1120-1180] | liquid | 500 [260] | B |
| F 58 | solution treat and quench | 2085 [1140] | liquid | 500 [260] | B |
| F 62 | solution treat and quench | 2025 [1105] | liquid | 500 [260] | B |
| F 63 | solution treat and quench | 1900 [1040] | liquid | 500 [260] | B |
| F 64 | solution treat and quench | 2010-2140 [1100-1170] | liquid | 500 [250] | B |
| F 904L | solution treat and quench | 1920-2100 [1050-1150] | liquid | 500 [260] | B |
| Ferritic-Austenitic Stainless Steels | |||||
| F 50 | solution treat and quench | 1925 [1050] | liquid | 500 [260] | B |
| F 51 | solution treat and quench | 1870 [1020] | liquid | 500 [260] | B |
| F 52C | liquid | 500 [260] | B | ||
| F 53 | solution treat and quench | 1880 [1025] | liquid | 500 [260] | B |
| F 54 | solution treat and quench | 1920-2060 [1050-1125] | liquid | 500 [260] | B |
| F 55 | solution treat and quench | 2010-2085 [1100-1140] | liquid | 500 [260] | B |
| F 57 | solution treat and quench | 1940 [1060] | liquid | 175 [80] | B |
| F 59 | solution treat and quench | 1975-2050 [1080-1120] | liquid | 500 [260] | B |
| F 60 | solution treat and quench | 1870 [1020] | liquid | 500 [260] | B |
| F 61 | solution treat and quench | 1920-2060 [1050-1125] | liquid | 500 [260] | B |
| F 65 | solution treat and quench | 1830-2100 [1000-1150] | liquidD | 500 [260] | B |
| F 66 | solution treat and quench | 1870-1975 [1020-1080] | liquid | 500 [260] | B |
| F 67 | solution treat and quench | 1870-2050 [1020-1120] | liquid | 500 [260] | B |
8 Chemical Composition
8.1 A chemical heat analysis in accordance with Specification A961/A961M shall be made and conform to the chemical composition prescribed in Table 2.
8.2 Grades to which lead, selenium, or other elements are added for the purpose of rendering the material free-machining shall not be used.
8.3 Starting material produced to a specification that specifically requires the addition of any element beyond those listed in Table 2 for the applicable grade of material is not permitted.
8.4 Steel grades covered in this specification shall not contain an unspecified element, other than nitrogen in stainless steels, for the ordered grade to the extent that the steel conforms to the requirements of another grade for which that element is a specified element having a required minimum content. For this requirement, a grade is defined as an alloy described individually and identified by its own UNS designation or Grade designation and identification symbol in Table 2.
8.5 Product Analysis—The purchaser may make a product analysis on products supplied to this specification in accordance with Specification A961/A961M.
9 Mechanical Properties
9.1 The material shall conform to the requirements as to mechanical properties for the grade ordered as listed in Table 3.
9.2 Mechanical test specimens shall be obtained from production forgings, or from separately forged test blanks pre-pared from the stock used to make the finished product. In either case, mechanical test specimens shall not be removed until after all heat treatment is complete. If repair welding is required, test specimens shall not be removed until after post-weld heat treatment is complete, except for ferritic grades when the post-weld heat treatment is conducted at least 50 °F [30 °C] below the actual tempering temperature. When test blanks are used, they shall receive approximately the same working as the finished product. The test blanks shall be heat treated with the finished product and shall approximate the maximum cross section of the forgings they represent.
9.3 For normalized and tempered, or quenched and tempered forgings, the central axis of the test specimen shall correspond to the 1⁄4 T plane or deeper position where T is the maximum heat-treated thickness of the represented forging. In addition, for quenched and tempered forgings, the mid-length of the test specimen shall be at least T from any second heat-treated surface. When the section thickness does not permit this positioning, the test specimen shall be positioned as near as possible to the prescribed location, as agreed to by the purchaser and the supplier.
9.3.1 With prior purchase approval, the test specimen for ferritic steel forgings may be taken at a depth (t) corresponding to the distance from the area of significant stress to the nearest heat-treated surface and at least twice this distance (2 t) from any second surface. However, the test depth shall not be nearer to one treated surface than 3⁄4 in. [19 mm] and to the second treated surface than 1
1
⁄2 in. [38 mm]. This method of test specimen location would normally apply to contour-forged parts, or parts with thick cross-sectional areas where 1⁄4 T 3
T testing (see 9.3) is not practical. Sketches showing the exact test locations shall be approved by the purchaser when this method is used.
9.3.2 Metal Buffers—The required distances from heattreated surfaces may be obtained with metal buffers instead of integral extensions. Buffer material may be carbon or low-alloy steel, and shall be joined to the forging with a partial penetration weld that seals the buffered surface. Specimens shall be located at 1
⁄2-in. [13-mm] minimum from the buffered surface of the forging. Buffers shall be removed and the welded areas subjected to magnetic particle test to ensure freedom from cracks unless the welded areas are completely removed by subsequent machining.
9.4 For annealed low alloy steels, ferritic stainless steels, and martensitic stainless steels, and also for austenitic and ferritic-austenitic stainless steels, the test specimen may be taken from any convenient location.
9.5 Tension Tests:
9.5.1 Low Alloy Steels and Ferritic and Martensitic Stainless Steels—One tension test shall be made for each heat in each heat treatment charge.
9.5.1.1 When the heat-treating cycles are the same and the furnaces (either batch or continuous type) are controlled within ±25°F [(±14°C)] and equipped with recording pyrometers so that complete records of heat treatment are available, then only one tension test from each heat of each forging type (see Note 1) and section size is required, instead of one test from each heat in each heat-treatment charge. NOTE 1—“Type” in this case is used to describe the forging shape such as a flange, ell, tee, and the like.
9.5.2 Austenitic and Ferritic-Austenitic Stainless Steel Grades—One tension test shall be made for each heat.
9.5.2.1 When heat treated in accordance with 7.1, the test blank or forging used to provide the test specimen shall be heat treated with a finished forged product.
9.5.2.2 When the alternative method in 7.3.1 is used, the test blank or forging used to provide the test specimen shall be forged and quenched under the same processing conditions as the forgings they represent.
9.5.3 Testing shall be performed in accordance with Test Methods and Definitions A370 using the largest feasible of the round specimens. The gage length for measuring elongation shall be four times the diameter of the test section.
9.6 Hardness Tests:
9.6.1 Except when only one forging is produced, a minimum of two pieces per batch or continuous run as defined in 9.6.2 shall be hardness tested in accordance with Test Methods and Definitions A370 to ensure that the forgings are within the hardness limits given for each grade in Table 3. The purchaser may verify that the requirement has been met by testing at any location on the forging provided such testing does not render the forging useless.
9.6.2 When the reduced number of tension tests permitted by 9.5.1.1 is applied, additional hardness tests shall be made on forgings or samples, as defined in 9.2, scattered throughout the load (see Note 2). At least eight samples shall be checked from each batch load, and at least one check per hour shall be made from a continuous run. When the furnace batch is less than
eight forgings, each forging shall be checked. If any check falls outside the prescribed limits, the entire lot of forgings shall be reheat treated and the requirements of 9.5.1 shall apply. NOTE 2—The tension test required in 9.5.1 is used to determine material capability and conformance in addition to verifying the adequacy of the heat-treatment cycle. Additional hardness tests in accordance with 9.6.2 are required when 9.5.1.1 is applied to ensure the prescribed heat-treating cycle and uniformity throughout the load.
9.6.3 When the alternative to the Ti/N ratio limit for F23 is applied, (see Note P in Table 2), a minimum of two pieces per batch or continuous run as defined in 9.6.2 shall be hardness tested, in the hardened condition (see 3.2.1), to ensure that the
forgings are within the hardness limit given for F23 in Note P of Table 2. The test samples shall be taken at the mid thickness of the thickest section of the product. Testing shall be performed in accordance with the Test Method E92 or with Test Methods and Definitions A370.
9.7 Notch Toughness Requirements—Grades F 3V, F 3VCb, and F 22V.
9.7.1 Impact test specimens shall be Charpy V-notch Type, as shown in Fig. 11a of Test Methods and Definitions A370. The usage of subsize specimens due to material limitations must have prior purchaser approval.
| Identification Symbol | UNS Designation | Grade | Composition, % | ||||||||||
| Carbon | Manganese | Phosphorus | Sulfur | Silicon | Nickel | Chromium | Molybdenum | Columbium | Titanium | Other Elements | |||
| Low Alloy Steels | |||||||||||||
| F 1 | K12822 | carbon-molybdenum | 0.28 | 0.60–0.90 | 0.045 | 0.045 | 0.15–0.35 | ... | ... | 0.44–0.65 | ... | ... | ... |
| F 2B | K12122 | 0.5 % chromium, 0.5 % molybdenum | 0.05–0.21 | 0.30–0.80 | 0.040 | 0.040 | 0.10–0.60 | ... | 0.50–0.81 | 0.44–0.65 | ... | ... | ... |
| F 5C | K41545 | 4 to 6 % chromium | 0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50 | 0.50 | 4.0–6.0 | 0.44–0.65 | ... | ... | ... |
| F 5aC | K42544 | 4 to 6 % chromium | 0.25 | 0.60 | 0.040 | 0.030 | 0.50 | 0.50 | 4.0–6.0 | 0.44–0.65 | ... | ... | ... |
| F 9 | K90941 | 9 % chromium | 0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50–1.00 | ... | 8.0–10.0 | 0.90–1.10 | ... | ... | ... |
| F 10 | S33100 | 20 nickel, 8 chromium | 0.10–0.20 | 0.50–0.80 | 0.040 | 0.030 | 1.00–1.40 | 19.0–22.0 | 7.0–9.0 | ... | ... | ... | ... |
| F 91 | K90901 | 9 % chromium, 1 % molybdenum, 0.2 % vanadium plus columbium and nitrogen | 0.08–0.12 | 0.30–0.60 | 0.020 | 0.010 | 0.20–0.50 | 0.40 | 8.0–9.5 | 0.85–1.05 | 0.06–0.10 | ... | N 0.03–0.07Al 0.02DV 0.18–0.25Ti 0.01DZr 0.01D |
| F 92 | K92460 | 9 % chromium, 1.8 % tungsten, 0.2 % vanadium plus columbium | 0.07–0.13 | 0.30–0.60 | 0.020 | 0.010 | 0.50 | 0.40 | 8.50–9.50 | 0.30–0.60 | 0.04–0.09 | ... | V 0.15–0.25N0.030–0.070Al 0.02DW 1.50–2.00B0.001–0.006Ti 0.01DZr 0.01D |
| F 122 | K91271 | 11 % chromium, 2 % tungsten, 0.2 % vanadium, plus molybdenum, columbium, copper, nickel, nitrogen, and boron | 0.07–0.14 | 0.70 | 0.020 | 0.010 | 0.50 | 0.50 | 10.00–11.50 | 0.25–0.60 | 0.04–0.10 | ... | V 0.15–0.30B 0.005N 0.040–0.100Al 0.02DCu 0.30–1.70W 1.50–2.50Ti 0.01DZr 0.01D |
| F 911 | K91061 | 9 % chromium, 1 % molybdenum, 0.2 % vanadium plus columbium and nitrogen | 0.09–0.13 | 0.30–0.60 | 0.020 | 0.010 | 0.10–0.50 | 0.40 | 8.5–9.5 | 0.90–1.10 | 0.060–0.10 | ... | W 0.90–1.10Al 0.02DN 0.04–0.09V 0.18–0.25B 0.0003–0.006Ti 0.01DZr 0.01D |
| F 11Class 1 | K11597 | 1.25 % chromium, 0.5 % molybdenum | 0.05–0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50–1.00 | ... | 1.00–1.50 | 0.44–0.65 | ... | ... | ... |
| F 11Class 2 | K11572 | 1.25 % chromium, 0.5 % molybdenum | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.50–1.00 | ... | 1.00–1.50 | 0.44–0.65 | ... | ... | ... |
| F 11Class 3 | K11572 | 1.25 % chromium, 0.5 % molybdenum | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.50–1.00 | ... | 1.00–1.50 | 0.44–0.65 | ... | ... | ... |
| F 12Class 1 | K11562 | 1 % chromium, 0.5 % molybdenum | 0.05–0.15 | 0.30–0.60 | 0.045 | 0.045 | 0.50 max | ... | 0.80–1.25 | 0.44–0.65 | ... | ... | ... |
| F 12Class 2 | K11564 | 1 % chromium, 0.5 % molybdenum | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.10–0.60 | ... | 0.80–1.25 | 0.44–0.65 | ... | ... | ... |
| F 21 | K31545 | chromium-molybdenum | 0.05–0.15 | 0.30–0.60 | 0.040 | 0.040 | 0.50 max | ... | 2.7–3.3 | 0.80–1.06 | ... | ... | ... |
A182/A182M-11
| Identification Symbol | UNS Designation | Grade | Composition, % | ||||||||||
| Carbon | Manganese | Phosphorus | Sulfur | Silicon | Nickel | Chromium | Molybdenum | Columbium | Titanium | Other Elements | |||
| F 3V | K31830 | 3 % chromium, 1 % molybdenum, 0.25 % vanadium plus boron and titanium | 0.05–0.18 | 0.30–0.60 | 0.020 | 0.020 | 0.10 | ... | 2.8–3.2 | 0.90–1.10 | ... | 0.015–0.035 | V 0.20–0.30 B 0.001–0.003 |
| F 3VCb | K31390 | 3 % chromium, 1 % molybdenum, 0.25 % vanadium plus boron, columbium, and titanium | 0.10–0.15 | 0.30–0.60 | 0.020 | 0.010 | 0.10 | 0.25 | 2.7–3.3 | 0.90–1.10 | 0.015–0.070 | 0.015 | V 0.20–0.30 Cu 0.25 Ca 0.0005–0.0150 |
| F 22 Class 1 | K21590 | chromium-molybdenum | 0.05–0.15 | 0.30–0.60 | 0.040 | 0.040 | 0.50 | ... | 2.00–2.50 | 0.87–1.13 | ... | ... | ... |
| F 22 Class 3 | K21590 | chromium-molybdenum | 0.05–0.15 | 0.30–0.60 | 0.040 | 0.040 | 0.50 | ... | 2.00–2.50 | 0.87–1.13 | ... | ... | ... |
| F 22V | K31835 | 2.25 % chromium, 1 % molybdenum, 0.25 % vanadium | 0.11–0.15 | 0.30–0.60 | 0.015 | 0.010 | 0.10 | 0.25 | 2.00–2.50 | 0.90–1.10 | 0.07 | 0.030 | Cu 0.20 V 0.25–0.35 B 0.002 Ca 0.015E |
| F 23 | K41650 | 2.25 % chromium, 1.6 % tungsten, 0.25 % vanadium, plus molybdenum, columbium, and boron | 0.04–0.10 | 0.10–0.60 | 0.030 | 0.010 | 0.50 | 0.40 | 1.90-2.60 | 0.05-0.30 | 0.02–0.08 | 0.005–0.060F | V 0.20–0.30 B 0.0010–0.006 N 0.015F Al 0.030 W 1.45–1.75 |
| F 24 | K30736 | 2.25 % chromium, 1 % molybdenum, 0.25 % vanadium plus titanium and boron | 0.05–0.10 | 0.30–0.70 | 0.020 | 0.010 | 0.15–0.45 | ... | 2.20–2.60 | 0.90–1.10 | ... | 0.06-0.10 | V 0.20–0.30 N 0.12 Al 0.020 B 0.0015–0.0070 |
| FR | K22035 | 2 % nickel, 1 % copper | 0.20 | 0.40–1.06 | 0.045 | 0.050 | ... | 1.60–2.24 | ... | ... | ... | ... | Cu 0.75–1.25 N 0.020 Al 0.050 Cu 0.50–0.80 V 0.02 |
| F 36 | K21001 | 1.15 % nickel, 0.65 % copper, molybdenum, and columbium | 0.10–0.17 | 0.80–1.20 | 0.030 | 0.025 | 0.25–0.50 | 1.00–1.30 | 0.30 | 0.25–0.50 | 0.015–0.045 | ... | ... |
| Martensitic Stainless Steels | |||||||||||||
| F 6a | S41000 | 13 % chromium 410G | 0.15 | 1.00 | 0.040 | 0.030 | 1.00 | 0.50 | 11.5–13.5 | ... | ... | ... | ... |
| F 6b | S41026 | 13 % chromium, 0.5 % molybdenum | 0.15 | 1.00 | 0.020 | 0.020 | 1.00 | 1.00–2.00 | 11.5–13.5 | 0.40–0.60 | ... | ... | Cu 0.50 |
| F 6NM | S41500 | 13 % chromium, 4 % nickel | 0.05 | 0.50–1.00 | 0.030 | 0.030 | 0.60 | 3.5–5.5 | 11.5–14.0 | 0.50–1.00 | ... | ... | ... |
| Ferritic Stainless Steels | |||||||||||||
| F XM-27CbH | S44627 | 27 chromium, 1 molybdenum XM-27G | 0.010 | 0.40 | 0.020 | 0.020 | 0.40 | 0.50 | 25.0–27.5 | 0.75–1.50 | 0.05–0.20 | N 0.015 Cu 0.20 | |
| F 429 | S42900 | 15 chromium 429G | 0.12 | 1.00 | 0.040 | 0.030 | 0.75 | 0.50 | 14.0–16.0 | ... | ... | ... | ... |
| F 430 | S43000 | 17 chromium 430G | 0.12 | 1.00 | 0.040 | 0.030 | 0.75 | 0.50 | 16.0–18.0 | ... | ... | ... | ... |
| Austenitic Stainless Steels | |||||||||||||
| F 304I | S30400 | 18 chromium, 8 nickel 304G | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 8.0–11.0 | 18.0–20.0 | ... | ... | ... | ... |
A182/A182M-11
| Identification Symbol | UNS Designation | Grade | Composition, % | ||||||||||
| Carbon | Manganese | Phosphorus | Sulfur | Silicon | Nickel | Chromium | Molybdenum | Columbium | Titanium | Other Elements | |||
| 304H | S30409 | 18 chromium, 8 nickel 304HG | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 8.0–11.0 | 18.0–20.0 | ... | ... | ... | ... |
| 304LI | S30403 | 18 chromium, 8 nickel, low carbon 304LG | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 8.0–13.0 | 18.0–20.0 | ... | ... | ... | ... |
| 304NJ | S30451 | 18 chromium, 8 nickel, modified with nitrogen 304NG | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 8.0–10.5 | 18.0–20.0 | ... | ... | ... | ... |
| 304LNJ | S30453 | 18 chromium, 8 nickel, modified with nitrogen 304LNG | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 8.0–10.5 | 18.0–20.0 | ... | ... | ... | ... |
| 309H | S30909 | 23 chromium, 13.5 nickel 309HG | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 12.0–15.0 | 22.0–24.0 | ... | ... | ... | ... |
| 310 | S31000 | 25 chromium, 20 nickel 310G | 0.25 | 2.00 | 0.045 | 0.030 | 1.00 | 19.0–22.0 | 24.0–26.0 | ... | ... | ... | ... |
| 310H | S31009 | 25 chromium, 20 nickel 310HG | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 19.0–22.0 | 24.0–26.0 | ... | ... | ... | ... |
| 10MoLN | S31050 | 25 chromium, 22 nickel, modified with molybdenum and nitrogen, low carbon 310MoLNG | 0.030 | 2.00 | 0.030 | 0.015 | 0.40 | 21.0–23.0 | 24.0–26.0 | 2.00–3.00 | ... | ... | N 0.10–0.16 |
| 316I | S31600 | 18 chromium, 8 nickel, modified with molybdenum 316G | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 10.0–14.0 | 16.0–18.0 | 2.00–3.00 | ... | ... | ... |
| 316H | S31609 | 18 chromium, 8 nickel, modified with molybdenum 316HG | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 10.0–14.0 | 16.0–18.0 | 2.00–3.00 | ... | ... | ... |
| 316LI | S31603 | 18 chromium, 8 nickel, modified with molybdenum, low carbon 316LG | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 10.0–15.0 | 16.0–18.0 | 2.00–3.00 | ... | ... | ... |
| 316NJ | S31651 | 18 chromium, 8 nickel, modified with molybdenum and nitrogen 316NG | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 11.0–14.0 | 16.0–18.0 | 2.00–3.00 | ... | ... | ... |
| 316LNJ | S31653 | 18 chromium, 8 nickel, modified with molybdenum and nitrogen 316LNG | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 11.0–14.0 | 16.0–18.0 | 2.00–3.00 | ... | ... | ... |
| 316Ti | S31635 | 18 chromium, 8 nickel, modified with molybdenum and nitrogen 316Ti | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 10.0–14.0 | 16.0–18.0 | 2.00–3.00 | ... | K | N 0.10 max |
| 317 | S31700 | 19 chromium, 13 nickel, 3.5 molybdenum 317G | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 11.0–15.0 | 18.0–20.0 | 3.0–4.0 | ... | ... | ... |
A182/A182M-11
| Identifi-cation Symbol | U NS Desig-nation | G rade |
| F 31 7L | S31 703 | 1 9 ch romium , 1 3 nickel , 3.5 molybdenum 31 7LG |
| S31 727 | S31 727 | 1 8 ch romium , 1 5 nickel , 4.5 molybdenum , 3.5 copper with nitrogen |
| S32053 | S32053 | 23 ch romium , 25 nickel , 5.5 molybdenum , with nitrogen |
| F 32 1 | S32 1 00 | 1 8 ch romium , 8 nickel modified with titanium 32 1 G |
| F 32 1 H | S32 1 09 | 1 8 ch romium , 8 nickel , modified with titanium 32 1 H G |
| F 347 | S34700 | 1 8 ch romium , 8 nickel modified with columbium347G |
| F 347H | S34709 | 1 8 ch romium , 8 nickel , modified with columbium 347H G |
| F347LN | S3475 1 | 1 8 ch romium , 8 nickel modified with columbium and nitrogen347LN |
| F 348 | S34800 | 1 8 ch romium , 8 nickel modified with columbium348G |
| F 348H | S34809 | 1 8 ch romium , 8 nickel , modified with columbium 348H G |
| F XM- 1 1 | S2 1 904 | 20 ch romium , 6 nickel , 9 manganese XM- 1 1 G |
| F XM- 1 9 | S209 1 0 | 22 ch romium , 1 3 nickel , 5 manganese XM- 1 9G |
| F 20 | N08020 | 35 nickel , 20 ch romium , 3.5 copper, 2.5 molybdenum |
| F 44 | S31 254 | 20 ch romium , 1 8 nickel , 6 molybdenum , low carbon |
| F 45 | S3081 5 | 2 1 ch romium , 1 1 nickel modified with nitrogen and cerium |
| Com | position , % | |||||||||
| Carbon | Manga-nese | Phos-phorus | Sulfu r | Silicon | N ickel | Ch romium | Molybde-num | Colum-bium | Titan-ium | Other Elements |
| 0.030 | 2.00 | 0.045 | 0.030 | 1 .00 | 1 1 .0-1 5.0 | 1 8.0-20.0 | 3.0-4.0 | . . . | . . . | . . . |
| 0.030 | 1 .00 | 0.030 | 0.030 | 1 .00 | 1 4.5-1 6.5 | 1 7.5-1 9.0 | 3.8-4.5 | . . . | . . . | Cu 2.8-4.0 N 0. 1 5-0.2 1 |
| 0.030 | 1 .00 | 0.030 | 0.01 0 | 1 .00 | 24.0-28.0 | 22.0-24.0 | 5.0-6.0 | . . . | . . . | N 0. 1 7-0.22 |
| 0.08 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 2.0 | 1 7.0-1 9.0 | . . . | . . . | L | . . . |
| 0.04-0. 1 0 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 2.0 | 1 7.0-1 9.0 | . . . | . . . | M | . . . |
| 0.08 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 3.0 | 1 7.0-20.0 | . . . | N | . . . | . . . |
| 0.04-0. 1 0 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 3.0 | 1 7.0-20.0 | . . . | O | . . . | . . . |
| 0.005-0.020 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 3.0 | 1 7.0-1 9.0 | . . . | 0.20-0.50P | . . . | N 0.06-0. 1 0 |
| 0.08 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 3.0 | 1 7.0-20.0 | . . . | N | . . . | Co 0.20 Ta 0. 1 0 |
| 0.04-0. 1 0 | 2.00 | 0.045 | 0.030 | 1 .00 | 9.0-1 3.0 | 1 7.0-20.0 | . . . | O | . . . | Co 0.20 Ta 0. 1 0 |
| 0.040 | 8.0-1 0.0 | 0.060 | 0.030 | 1 .00 | 5.5-7.5 | 1 9.0-2 1 .5 | . . . | . . . | . . . | N 0. 1 5-0.40 |
| 0.06 | 4.0-6.0 | 0.040 | 0.030 | 1 .00 | 1 1 .5-1 3.5 | 20.5-23.5 | 1 .50-3.00 | 0. 1 0-0.30 | . . . | N 0.20-0.40 V 0. 1 0-0.30 |
| .07 | 2.00 | 0.045 | 0.035 | 1 .00 | 32.0-38.0 | 1 9.0-2 1 .0 | 2.00-3.00 | 8xCmin-1 .00 | . . . | Cu 3.0-4.0 |
| 0.020 | 1 .00 | 0.030 | 0.01 0 | 0.80 | 1 7.5-1 8.5 | 1 9.5-20.5 | 6.0-6.5 | . . . | . . . | Cu 0.50-1 .00 N 0. 1 8-0.22 |
| 0.05-0. 1 0 | 0.80 | 0.040 | 0.030 | 1 .40-2.00 | 1 0.0-1 2.0 | 20.0-22.0 | . . . | . . . | . . . | N 0. 1 4-0.20 Ce 0.03-0.08 |
A182/A182M - 11
| Identifi-cation Symbol | U NS Desig-nation | G rade |
| F 46 | S30600 | 1 8 ch romium , 1 5 nickel , 4 silicon |
| F 47 | S31 725 | 1 9 ch romium , 1 5 nickel , 4 molybdenum 31 7LM G |
| F 48 | S31 726 | 1 9 ch romium , 1 5 nickel , 4 molybdenum 31 7LM N G |
| F 49 | S34565 | 24 ch romium , 1 7 nickel , 6 manganese, 5 molybdenum |
| F 56 | S33228 | 32 nickel , 27 ch romium with columbium |
| F 58 | S31 266 | 24 ch romium , 20 nickel , 6 molybdenum , 2 tungsten with nitrogen |
| F 62 | N08367 | 2 1 ch romium , 25 nickel , 6.5 molybdenum |
| F 63 | S3261 5 | 1 8 ch romium , 20 nickel , 5.5 silicon |
| F 64 | S30601 | 1 7.5 ch romium , 1 7.5 nickel , 5.3 silicon |
| F 904L | N08904 | 2 1 ch romium , 26 nickel , 4.5 molybdenum 904LG |
| F 50 | S31200 | 25 chromium, 6 nickel, modified with nitrogen |
| F 51 | S31803 | 22 chromium, 5.5 nickel, modified with nitrogen |
| F 52 | S32950 | 26 chromium, 3.5 nickel, 1.0 molybdenum |
| F 53 | S32750 | 25 chromium, 7 nickel, 4 molybdenum, modified with nitrogen 2507G |
| F 54 | S39274 | 25 chromium, 7 nickel, modified with nitrogen and tungsten |
| F 55 | S32760 | 25 chromium, 7 nickel, 3.5 molybdenum, modified with nitrogen and tungsten |
| F 57 | S39277 | 26 chromium, 7 nickel, 3.7 molybdenum |
| F 59 | S32520 | 25 chromium, 6.5 nickel, 4 molybdenum with nitrogen |
| Composition, % | ||||||||||
| Carbon | Manganese | Phosphorus | Sulfur | Silicon | Nickel | Chromium | Molybdenum | Columbium | Titanium | Other Elements |
| 0.018 | 2.00 | 0.020 | 0.020 | 3.7–4.3 | 14.0–15.5 | 17.0–18.5 | 0.20 | ... | ... | Cu 0.50 |
| 0.030 | 2.00 | 0.045 | 0.030 | 0.75 | 13.0–17.5 | 18.0–20.0 | 4.0–5.0 | ... | ... | N 0.10 |
| 0.030 | 2.00 | 0.045 | 0.030 | 0.75 | 13.5–17.5 | 17.0–20.0 | 4.0–5.0 | ... | ... | N 0.10–0.20 |
| 0.030 | 5.0–7.0 | 0.030 | 0.010 | 1.00 | 16.0–18.0 | 23.0–25.0 | 4.0–5.0 | 0.10 | ... | N 0.40–0.60 |
| 0.04–0.08 | 1.00 | 0.020 | 0.015 | 0.30 | 31.0–33.0 | 26.0–28.0 | ... | 0.6–1.0 | ... | Ce 0.05–0.10Al 0.025 |
| 0.030 | 2.0–4.0 | 0.035 | 0.020 | 1.00 | 21.0–24.0 | 23.0–25.0 | 5.2–6.2 | ... | ... | N 0.35–0.60Cu 1.00–2.50W 1.50–2.50 |
| 0.030 | 2.00 | 0.040 | 0.030 | 1.00 | 23.5–25.5 | 20.0–22.0 | 6.0–7.0 | ... | ... | N 0.18–0.25Cu 0.75 |
| 0.07 | 2.00 | 0.045 | 0.030 | 4.8-6.0 | 19.0-22.0 | 16.5-19.5 | 0.30-1.50 | ... | ... | Cu 1.50-2.50 |
| 0.015 | 0.50-0.80 | 0.030 | 0.013 | 5.0-5.6 | 17.0-18.0 | 17.0-18.0 | 0.20 | ... | ... | Cu 0.35, N 0.05 |
| 0.020 | 2.0 | 0.040 | 0.030 | 1.00 | 23.0–28.0 | 19.0–23.0 | 4.0–5.0 | ... | ... | Cu 1.00–2.00N 0.10 |
| Fer | ritic-Austeni | tic Stainless | Steels | |||||||
| 0.030 | 2.00 | 0.045 | 0.030 | 1 .00 | 5.5-6.5 | 24.0-26.0 | 1 .20-2.00 | . . . | . . . | N 0. 1 4-0.20 |
| 0.030 | 2.00 | 0.030 | 0.020 | 1 .00 | 4.5-6.5 | 2 1 .0-23.0 | 2.5-3.5 | . . . | . . . | N 0.08-0.20 |
| 0.030 | 2.00 | 0.035 | 0.01 0 | 0.60 | 3.5-5.2 | 26.0-29.0 | 1 .00-2.50 | . . . | . . . | N 0. 1 5-0.35 |
| 0.030 | 1 .20 | 0.035 | 0.020 | 0.80 | 6.0-8.0 | 24.0-26.0 | 3.0-5.0 | . . . | . . . | N 0.24-0.32 Cu 0.50 |
| 0.030 | 1 .00 | 0.030 | 0.020 | 0.80 | 6.0-8.0 | 24.0-26.0 | 2.5-3.5 | . . . | . . . | N 0.24-0.32 Cu 0.20-0.80 W 1 .50-2.50 |
| 0.030 | 1 .00 | 0.030 | 0.01 0 | 1 .00 | 6.0-8.0 | 24.0-26.0 | 3.0-4.0 | . . . | . . . | N 0.20-0.30 Cu 0.50-1 .00 W 0.50-1 .00Q |
| 0.025 | 0.80 | 0.025 | 0.002 | 0.80 | 6.5-8.0 | 24.0-26.0 | 3.0-4.0 | . . . | . . . | Cu 1 .20-2.00 W 0.80-1 .20 N 0.23-0.33 |
| 0.030 | 1 .50 | 0.035 | 0.020 | 0.80 | 5.5-8.0 | 24.0-26.0 | 3.0-5.0 | . . . | . . . | N 0.20-0.35 Cu 0.50-3.00 |
A182/A182M-11
| Identification Symbol | UNS Designation | Grade | Composition, % | ||||||||||
| Carbon | Manganese | Phosphorus | Sulfur | Silicon | Nickel | Chromium | Molybdenum | Columbium | Titanium | Other Elements | |||
| F 60 | S32205 | 22 chromium, 5.5 nickel, 3 molybdenum, modified with nitrogen 2205G | 0.030 | 2.00 | 0.030 | 0.020 | 1.00 | 4.5–6.5 | 22.0–23.0 | 3.0–3.5 | ... | ... | N 0.14–0.20 |
| F 61 | S32550 | 26 chromium, 6 nickel, 3.5 molybdenum with nitrogen and copper 255G | 0.040 | 1.50 | 0.040 | 0.030 | 1.00 | 4.5–6.5 | 24.0–27.0 | 2.9–3.9 | ... | ... | Cu 1.50–2.50N 0.10–0.25 |
| F 65 | S32906 | 29 chromium, 6.5 nickel, 2 molybdenum with nitrogen | 0.030 | 0.80–1.50 | 0.030 | 0.030 | 0.80 | 5.8–7.5 | 28.0–30.0 | 1.5–2.6 | ... | ... | Cu 0.80N 0.30–0.40 |
| F 66 | S32202 | 22 chromium, 2.0 nickel, 0.25 molybdenum with nitrogen | 0.030 | 2.00 | 0.040 | 0.010 | 1.00 | 1.00–2.80 | 21.5–24.0 | 0.45 | ... | ... | N 0.18–0.26 |
| F 67 | S32506 | 25 chromium, 6 nickel, 3 molybdenum, with nitrogen and tungsten | 0.030 | 1.00 | 0.040 | 0.015 | 0.90 | 5.5–7.2 | 24.0–26.0 | 3.0–3.5 | ... | ... | N 0.08–0.20W 0.05–0.30 |
D
Appl ies to both heat and p rod uct analyses .
G Nam i ng system developed and appl ied by ASTM .
H G rade F XM -27Cb shal l have a n ickel pl us coppe r content of 0 . 50 max % . P rod uct analysis tole rance ove r the maxi m u m specified l i m it fo r carbon and n itrogen shal l be 0 . 002 % .
I G rades F 304 , F 304 L, F 3 1 6 , and F 3 1 6 L shal l have a maxi m u m n itrogen content of 0 . 1 0 % .
J G rades F 304 N , F 3 1 6 N , F 304 LN , and F 3 1 6 LN shal l have a n itrogen content of 0 . 1 0 to 0 . 1 6 % .
K G rade F 3 1 6Ti shal l have a titan i u m content not l ess than five ti mes the carbon pl us n itrogen content and not mo re than 0 . 70 % .
L G rade F 32 1 shal l have a titan i u m content of not l ess than five ti mes the carbon content and not mo re than 0 . 70 % .
M G rade F 32 1 H shal l have a titan i u m content of not l ess than fou r ti mes the carbon content and not mo re than 0 . 70 % .
N G rades F 347 and F 348 shal l have a col u m bi u m content of not l ess than ten ti mes the carbon content and not mo re than 1 . 1 0 % .
O G rades F 347 H and F 348 H shal l have a col u m bi u m content of not l ess than e i g ht ti mes the carbon content and not mo re than 1 . 1 0 % .
P
G rade F347 LN shal l have a col u m bi u m content of not l ess than 1 5 ti mes the carbon content .
Q % C r + 3 . 3 3 % M o + 1 6 3 % N = 40 m i n .
A182/A182M-11
| Grade Symbol | Tensile Strength, min, ksi [MPa] | Yield Strength, min, ksi [MPa]B | Elongation in 2 in. [50 mm] or 4D, min, % | Reduction of Area, min, % | Brinell Hardness Number, HBW |
| Low Alloy Steels | |||||
| F 1 | 70 [485] | 40 [275] | 20 | 30 | 143-192 |
| F 2 | 70 [485] | 40 [275] | 20 | 30 | 143-192 |
| F 5 | 70 [485] | 40 [275] | 20 | 35 | 143-217 |
| F 5a | 90 [620] | 65 [450] | 22 | 50 | 187-248 |
| F 9 | 85 [585] | 55 [380] | 20 | 40 | 179-217 |
| F 10 | 80 [550] | 30 [205] | 30 | 50 | ... |
| F 91 | 90 [620] | 60 [415] | 20 | 40 | 190-248 |
| F 92 | 90 [620] | 64 [440] | 20 | 45 | 269 max |
| F 122 | 90 [620] | 58 [400] | 20 | 40 | 250 max |
| F 911 | 90 [620] | 64 [440] | 18 | 40 | 187-248 |
| F 11 Class 1 | 60 [415] | 30 [205] | 20 | 45 | 121-174 |
| F 11 Class 2 | 70 [485] | 40 [275] | 20 | 30 | 143-207 |
| F 11 Class 3 | 75 [515] | 45 [310] | 20 | 30 | 156-207 |
| F 12 Class 1 | 60 [415] | 32 [220] | 20 | 45 | 121-174 |
| F 12 Class 2 | 70 [485] | 40 [275] | 20 | 30 | 143-207 |
| F 21 | 75 [515] | 45 [310] | 20 | 30 | 156-207 |
| F 3V, and F 3VCb | 85-110 [585-760] | 60 [415] | 18 | 45 | 174-237 |
| F 22 Class 1 | 60 [415] | 30 [205] | 20 | 35 | 170 max |
| F 22 Class 3 | 75 [515] | 45 [310] | 20 | 30 | 156-207 |
| F 22V | 85-110 [585-780] | 60 [415] | 18 | 45 | 174-237 |
| F 23 | 74 [510] | 58 [400] | 20 | 40 | 220 max |
| F 24 | 85 [585] | 60 [415] | 20 | 40 | 248 max |
| FR | 63 [435] | 46 [315] | 25 | 38 | 197 max |
| F 36, Class 1 | 90 [620] | 64 [440] | 15 | ... | 252 max |
| F 36, Class 2 | 95.5 [660] | 66.5 [460] | 15 | ... | 252 max |
| Martensitic Stainless Steels | |||||
| F 6a Class 1 | 70 [485] | 40 [275] | 18 | 35 | 143-207 |
| F 6a Class 2 | 85 [585] | 55 [380] | 18 | 35 | 167-229 |
| F 6a Class 3 | 110 [760] | 85 [585] | 15 | 35 | 235-302 |
| F 6a Class 4 | 130 [895] | 110 [760] | 12 | 35 | 263-321 |
| F 6b | 110-135 [760-930] | 90 [620] | 16 | 45 | 235-285 |
| F 6NM | 115 [790] | 90 [620] | 15 | 45 | 295 max |
| Ferritic Stainless Steels | |||||
| F XM-27Cb | 60 [415] | 35 [240] | 20 | 45 | 190 max |
| F 429 | 60 [415] | 35 [240] | 20 | 45 | 190 max |
| F 430 | 60 [415] | 35 [240] | 20 | 45 | 190 max |
| Austenitic Stainless Steels | |||||
| F 304 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 304H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 304L | 70 [485]D | 25 [170] | 30 | 50 | ... |
| F 304N | 80 [550] | 35 [240] | 30E | 50F | ... |
| F 304LN | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 309H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 310 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 310MoLN | 78 [540] | 37 [255] | 25 | 40 | ... |
| F 310H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 316 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 316H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 316L | 70 [485]D | 25 [170] | 30 | 50 | ... |
| F 316N | 80 [550] | 35 [240] | 30E | 50F | ... |
| F 316LN | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 316Ti | 75 [515] | 30 [205] | 30 | 40 | ... |
| F 317 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 317L | 70 [485]D | 25 [170] | 30 | 50 | ... |
| S31727 | 80 [550] | 36 [245] | 35 | 50 | 217 |
| S32053 | 93 [640] | 43 [295] | 40 | 50 | 217 |
| F 347 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 347H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 347LN | 75 [515] | 30 [205] | 30 | 50 | ... |
| F 348 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 348H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 321 | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F 321H | 75 [515]C | 30 [205] | 30 | 50 | ... |
| F XM-11 | 90 [620] | 50 [345] | 45 | 60 | ... |
| Grade Symbol | Tensile Strength, min, ksi [MPa] | Yield Strength, min, ksi [MPa]B | Elongation in 2 in. [50 mm] or 4D, min, % | Reduction of Area, min, % | Brinell Hardness Number, HBW |
| F XM-19 | 100 [690] | 55 [380] | 35 | 55 | ... |
| F 20 | 80 [550] | 35 [240] | 30 | 50 | ... |
| F 44 | 94 [650] | 44 [300] | 35 | 50 | ... |
| F 45 | 87 [600] | 45 [310] | 40 | 50 | ... |
| F 46 | 78 [540] | 35 [240] | 40 | 50 | ... |
| F 47 | 75 [525] | 30 [205] | 40 | 50 | ... |
| F 48 | 80 [550] | 35 [240] | 40 | 50 | ... |
| F 49 | 115 [795] | 60 [415] | 35 | 40 | ... |
| F 56 | 73 [500] | 27 [185] | 30 | 35 | ... |
| F 58 | 109 [750] | 61 [420] | 35 | 50 | ... |
| F 62 | 95 [655] | 45 [310] | 30 | 50 | ... |
| F 63 | 80 [550] | 32 [220] | 25 | ... | 192 max |
| F 64 | 90 [620] | 40 [275] | 35 | 50 | 217 max |
| F 904L | 71 [490] | 31 [215] | 35 | ... | ... |
| Ferritic-Austenitic Stainless Steels | |||||
| F 50 | 100–130 [690–900] | 65 [450] | 25 | 50 | ... |
| F 51 | 90 [620] | 65 [450] | 25 | 45 | ... |
| F 52 | 100 [690] | 70 [485] | 15 | ... | ... |
| F 53 | 116 [800]G | 80 [550]G | 15 | ... | 310 max |
| F 54 | 116 [800] | 80 [550] | 15 | 30 | 310 max |
| F 55 | 109–130 [750–895] | 80 [550] | 25 | 45 | ... |
| F 57 | 118 [820] | 85 [585] | 25 | 50 | ... |
| F 59 | 112 [770] | 80 [550] | 25 | 40 | ... |
| F 60 | 95 [655] | 65 [450] | 25 | 45 | ... |
| F 61 | 109 [750] | 80 [550] | 25 | 50 | ... |
| F 65 | 109 [750] | 80 [550] | 25 | ... | ... |
| F 66 | 94 [650] | 65 [450] | 30 | ... | 290 max |
| F 67 | 90 [620] | 65 [450] | 18 | ... | 302 |
9.7.2 The Charpy V-notch test specimens shall be obtained as required for tension tests in 9.2, 9.3 and 9.5. One set of three Charpy V-notch specimens shall be taken from each tensile specimen location.
9.7.3 The longitudinal axis and mid-length of impact specimen shall be located similarly to the longitudinal axis of the tension test specimens. The axis of the notch shall be normal to the nearest heat-treated surface of the forging.
9.7.4 The Charpy V-notch tests shall meet a minimum energy absorption value of 40 ft-lbf [54 J] average of three specimens. One specimen only in one set may be below 40 ft-lbf [54 J], and it shall meet a minimum value of 35 ft-lbf [48 J].
9.7.5 The impact test temperature shall be 0°F [-18°C]
10 Grain Size for Austenitic Grades
10.1 All H grades and grade F 63 shall be tested for average grain size by Test Methods E112.
10.1.1 Grades F 304H, F 309H, F 310H, and F 316H shall have a grain size of ASTM No. 6 or coarser.
10.1.2 Grades F 321H, F 347H, and F 348H shall have a grain size of ASTM No. 7 or coarser.
10.1.3 Grade F 63 shall have a grain size of ASTM No. 3 or finer.
11 Corrosion Testing for Austenitic Grades
11.1 Corrosion testing is not required by this specification.
11.2 Austenitic grades shall be capable of meeting the intergranular corrosion test requirements described in Supplementary Requirement S4.
12 Retreatment
12.1 If the results of the mechanical tests do not conform to the requirements specified, the manufacturer may reheat treat the forgings and repeat the tests specified in Section 9.
13 Nondestructive Test Requirements
13.1 Hollow forgings of Grades F 91, F 92, F 122, and F 911, NPS 4 [DIN 100] and larger, whose internal surfaces are not accessible to magnetic particle or liquid penetrant examination, shall be examined by an ultrasonic test in accordance with Practice A388/A388M.
13.2 Hollow forgings of Grades F 91, F 92, F 122, and F 911, NPS 4 [DIN 100] and larger, whose internal surfaces are accessible to magnetic particle or liquid penetrant examination, shall be examined on their internal surfaces by either a magnetic particle test in accordance with Practice A275/ A275M, or by a liquid penetrant examination in accordance with Test Method E165, as applicable.
13.3 Time of Examination:
13.3.1 Examination by one of the methods in 13.1 or 13.2, for specification acceptance, shall be performed after all mechanical processing and heat treatment. This requirement does not preclude additional testing at earlier stages in the processing.
13.4 Evaluation of Imperfections Found by Ultrasonic Examination:
13.4.1 Forgings producing a signal equal to or greater than the lowest signal produced by the reference discontinuities shall be identified and separated from the acceptable forgings. The area producing the signal may be reexamined.
13.4.3 If the test signals were produced by visual imperfections such as scratches, surface roughness, dings, tooling marks, cutting chips, steel die stamps, or stop marks, the forging is permitted to be accepted based upon visual examination provided that the depth of the imperfection is less than 0.004 in. [0.1 mm] or 12.5 % of the specified wall thickness, whichever is the greater.
13.5 Treatment of Imperfections Found by Magnetic Particle or Liquid Penetrant Examination:
13.5.1 Defects shall be completely removed prior to weld repair by chipping or grinding to sound metal. Removal of these defects shall be verified by magnetic particle inspection in accordance with Test Method A275/A275M or by liquid penetrant inspection in accordance with Test Method E165.
13.5.2 Rejected forgings may be reconditioned and retested, provided that the wall thickness is not decreased to less than that required by this specification and the purchase order. The outside diameter at the point of grinding may be reduced by the amount so removed. To be accepted, retested forgings shall meet the test requirement.
13.5.3 If the imperfection is explored to the extent that it can be identified as non-rejectable, the forging may be accepted without further test provided that the imperfection does not encroach on the minimum required wall thickness.
14 Workmanship, Finish, and Appearance
14.1 Forgings shall conform to the requirements of Specification A961/A961M.
14.2 The forgings shall be free of scale, machining burrs which might hinder fit-up, and other injurious imperfections as defined herein. The forgings shall have a workmanlike finish,
and machined surfaces (other than surfaces having special requirements) shall have a surface finish not to exceed 250 AA (arithmetic average) roughness height.
15 Repair by Welding
15.1 Weld repairs shall be permitted (see Supplementary Requirement S58 of Specification A961/A961M) at the discretion of the manufacturer with the following limitations and requirements:
15.1.1 The welding procedure and welders shall be qualified in accordance with Section IX of the ASME Boiler and Pressure Vessel Code.
15.1.2 The weld metal shall be deposited using the electrodes specified in Table 4 except as otherwise provided in Supplementary Requirement S5. The electrodes shall be purchased in accordance with AWS Specifications A5.4/A5.4M, A5.5/A5.5M, A5.9/A5.9M, A5.11/A5.11M, A5.14/A5.14M, A5.23/A5.23M, A5.28/A5.28M, or A5.29/A5.29M. The submerged arc process with neutral flux, the gas metal-arc process, the gas tungsten-arc process, and gas shielded processes using flux-core consumables, may be used.
15.1.3 Defects shall be completely removed prior to welding by chipping or grinding to sound metal as verified by magnetic-particle inspection in accordance with Test Method A275/A275M for the low alloy steels and ferritic, martensitic, or ferritic-austenitic stainless steels, or by liquid-penetrant inspection in accordance with Test Method E165 for all grades.
15.1.4 After repair welding, the welded area shall be ground smooth to the original contour and shall be completely free of defects as verified by magnetic-particle or liquid-penetrant inspection, as applicable.
15.1.5 The preheat, interpass temperature, and post-weld heat treatment requirements given in Table 4 shall be met. Austenitic stainless steel forgings may be repair-welded without the post-weld heat treatment of Table 4, provided purchaser approval is obtained prior to repair.
15.1.6 Repair by welding shall not exceed 10 % of the surface area of the forging nor 33
1
⁄3 % of the wall thickness of the finished forging or 3
⁄8 in. [9.5 mm], whichever is less, without prior approval of the purchaser.
15.1.7 When approval of the purchaser is obtained, the limitations set forth in 15.1.6 may be exceeded, but all other requirements of Section 15 shall apply.
15.1.8 No weld repairs are permitted for F 6a Classes 3 and 4.
15.1.9 Post-weld heat treatment times for F 36 are: for Class 1, up to 2 in. [50 mm] in thickness, 1 h per in. [25 mm], 15 minutes minimum, and over 2 in. [50 mm], 15 minutes for each additional in. of thickness or fraction thereof; for Class 2, 1 h per in. [25 mm], 1⁄2 h minimum.
| Grade Symbol | ElectrodesA | Recommended Preheat and Interpass Temperature Range, °F [°C] | Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C] |
| Low Alloy Steels | |||
| F 1 | E 7018-A 1 | 200–400 [95–205] | 1150 [620] |
| F 2 | E 8018-B 1 | 300–600 [150–315] | 1150 [620] |
| Grade Symbol | ElectrodesA | Recommended Preheat and Interpass Temperature Range, °F [°C] | Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C] |
| F 5 | E80XX-B6, where XX can be 15, 16, or 18 | 400–700 [205–370] | 1250 [675] |
| F 5a | E80XX-B6, where XX can be 15, 16, or 18 | 400–700 [205–370] | 1250 [675] |
| F 9 | E80XX-B8, where XX can be 15, 16, or 18 | 400–700 [205–370] | 1250 [675] |
| F 10B | ... | ... | ... |
| F 91 | ...C | 400–700 [205–370] | 1350–1470 [730–800] |
| F 92 | ...D | 400–700 [205–370] | 1350–1470 [730–800] |
| F 122 | ...D | 400–700 [205–370] | 1350–1470 [730–800] |
| F 911 | ...D | 400–700 [205–370] | 1365–1435 [740–780] |
| F 11, Class 1, 2, and 3 | E 8018-B 2 | 300–600 [150–315] | 1150 [620] |
| F 12, Class 1 and 2 | E 8018-B 2 | 300–600 [150–315] | 1150 [620] |
| F 21 | E 9018-B 3 | 300–600 [150–315] | 1250 [675] |
| F 3V, and F 3VCb | 3 % Cr, 1 % Mo, 1⁄4 % V-Ti | 300–600 [150–315] | 1250 [675] |
| F 22 Class 1 | E 9018-B 3 | 300–600 [150–315] | 1250 [675] |
| F 22 Class 3 | E 9018-B 3 | 300–600 [150–315] | 1250 [675] |
| F 22V | 2.25 % Cr, 1 % Mo, 0.25 % V-Cb | 300–600 [150–315] | 1250 [675] |
| F 23 | 2.25 % Cr, 1.6 % W, 0.25 % V-Mo-Cb-B | 300-600 [150–315] | 1350–1470 [730–800] |
| F 24 | 2.25 % Cr, 1 % Mo, 0.25 % V | 200–400 [95–205]E | 1350–1470 [730–800]E |
| F 36, Class 1 | 1.15 Ni, 0.65 Cu, Mo, Cb | 400–700 [205–370] | 1100–1200 [595–650] |
| F 36, Class 2 | 1.15 Ni, 0.65 Cu, Mo, Cb | 400–700 [205–370] | 1000–1150 [540–620] |
| Martensitic Stainless Steels | |||
| F 6a, Class 1 | E 410-15 or 16 | 400–700 [205–370] | 1250 [675] |
| F 6a, Class 2 | E 410-15 or 16 | 400–700 [205–370] | 1250 [675] |
| F 6b | 13 % Cr, 11⁄2 % Ni, 1⁄2 % Mo | 400–700 [205–370] | 1150 [620] |
| F 6NM | 13 % Cr, 4 % Ni | 300–700 [150–370] | 1050 [565] |
| Ferritic Stainless Steels | |||
| F XM-27Cb | 26 % Cr, 1 % Mo | NRF | NR |
| F 429 | E 430-16 | 400–700 [205–370] | 1400 [760] |
| F 430 | E 430-16 | NR | 1400 [760] |
| FR | E 8018-C2 | NR | NR |
| Austenitic Stainless Steels | |||
| F 304 | E 308-15 or 16 | NR | 1900 [1040] + WQG |
| F 304L | E 308L-15 or 16 | NR | 1900 [1040] + WQ |
| F 304H | E 308-15 or 16H or E308H-XX | NR | 1900 [1040] + WQ |
| F 304N | E 308-15 or 16 | NR | 1900 [1040] + WQ |
| F 304LN | E 308L-15 or 16 | NR | 1900 [1040] + WQ |
| F 309H | E 309-15 or 16H or E309H-XX | NR | 1900 [1040] + WQ |
| F 310 | E 310-15 or 16 | NR | 1900 [1040] + WQ |
| F 310H | E 310-15 or 16H | NR | 1900 [1040] + WQ |
| F 310MoLN | E 310Mo-15 or 16 | NR | 1920–2010 [1050–1100] + WQ |
| F 316 | E 316-15 or 16 | NR | 1900 [1040] + WQ |
| F 316L | E 316L-15 or 16 | NR | 1900 [1040] + WQ |
| F 316H | E 316-15 or 16H or E316H-XX | NR | 1900 [1040] + WQ |
| F 316N | E 316-15 or 16 | NR | 1900 [1040] + WQ |
| F 316LN | E 316L-15 or 16 | NR | 1900 [1040] + WQ |
| F 316Ti | E 316-15 or 16 | NR | 1900 [1040] + WQ |
| F 317 | E 317-15 or 16 | NR | 1900 [1040] + WQ |
| F 317L | E 317L-15 or 16 | NR | 1900 [1040] + WQ |
| S31727 | ... | NR | ... |
| S32053 | ... | NR | ... |
| F 321B | E 347-15 or 16 | NR | 1900 [1040] + WQ |
| F 321HB | E 347-15 or 16H | NR | 1925 [1050] + WQ |
| F 347 | E 347-15 or 16 | NR | 1900 [1040] + WQ |
| F 347H | E 347-15 or 16H | NR | 1925 [1050] + WQ |
| F 347LNf | E 347-15 or 16 | NR | ... |
| E 348 | E 347-15 or 16 | NR | 1900 [1040] + WQ |
| F 348H | E 347-15 or 16H | NR | 1925 [1050] + WQ |
| F XM-11 | XM-10W | NR | NR |
| F XM-19 | XM-19W | NR | NR |
| F 20 | E/ER-320, 320LR | NR | 1700–1850 [925–1010] + WQ |
| F 44 | E NiCrMo-3 | NR | 2100 [1150] + WQ |
| F 45B | ... | ... | ... |
| F 46 | ... | ... | ... |
| F 47 | ...J | ... | 2100 [1150] + WQ |
| Grade Symbol | ElectrodesA | Recommended Preheat and Interpass Temperature Range, °F [°C] | Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C] |
| F 48 | ...J | ... | 2100 [1150] + WQ |
| F 49 | ...J | ... | 2100 [1150] + WQ |
| F 58 | E NiCrMo-10 | ... | 2100 [1150] + WQ |
| F 62 | E NiCrMo-3 | NR | 2025 [1105] + WQ |
| F 904L | E NiCrMo-3 | NR | 1920–2100 [1050–1150] + WQ |
| Ferritic-Austenitic Stainless Steels | |||
| F 50 | 25 % Cr, 6 % Ni, 1.7 % Mo | NR | NR |
| F 51 | 22 % Cr, 5.5 % Ni, 3 % Mo | NR | NR |
| F 52 | 26 % Cr, 8 % Ni, 2 % Mo | NR | NR |
| F 53 | 25 % Cr, 7 % Ni, 4 % Mo | NR | NR |
| F 54 | 25 % Cr, 7 % Ni, 3 % Mo, W | NR | NR |
| F 55 | 25 % Cr, 7 % Ni, 3.5 % Mo | NR | NR |
| F 57 | 25 % Cr, 7 % Ni, 3 % Mo, 1.5 % Cu, 1 % W | NR | NR |
| F 59 | E Ni CrMo-10 | NR | NR |
| F 60 | 22 % Cr, 5.5 % Ni, 3 % Mo | NR | NR |
| F 61 | 26 % Cr, 9 % Ni, 3.5 % Mo | NR | NR |
| F 65 | 29 % Cr, 6.5 % Ni, 2 % Mo | NR | NR |
| F 66 | 22 % Cr, 2 % Ni, 0.25 % Mo | NR | NR |
| F 67 | ... | NR | NR |
16 Inspection
16.1 Inspection provisions of Specification A961/A961M apply.
17 Rejection and Rehearing
17.1 The purchaser shall comply with the provisions of Specification A961/A961M.
18 Certification
18.1 In addition to the certification requirements of Specification A961/A961M, test reports shall be furnished to the purchaser or his representative.
18.2 Test reports shall include certification that all requirements of this specification have been met. The specification designation included on test reports shall include year of issue and revision letter, if any. The manufacturer shall provide the following where applicable:
18.2.1 Type heat treatment, Section 7,
18.2.2 Product analysis results, Section 8 of Specification A961/A961M,
18.2.3 Tensile property results, Section 9 (Table 3), report the yield strength and ultimate strength, in ksi [MPa], elongation and reduction in area, in percent,
18.2.4 Chemical analysis results, Section 8 (Table 2),
18.2.5 Hardness results, Section 9 (Table 3, and for F23, Tables 2 and 3),
18.2.6 Grain size results, Section 10, and
18.2.7 Any supplementary testing required by the purchase order.
19 Product Marking
19.1 In addition to the marking requirements of Specification A961/A961M, the manufacturer’s name (see Note 3) or symbol shall be permanently marked on each forging. NOTE 3—For purposes of identification marking, the manufacturer is considered the organization that certifies the piping component was manufactured, sampled, and tested in accordance with this specification, and the results have been determined to meet the requirements of this specification.
19.1.1 Quenched and tempered low alloy or martensitic stainless forgings shall be stamped with the letters QT following the specification designation.
19.1.2 Forgings repaired by welding shall be marked with the letter “W” following the Specification designation. When repair-welded austenitic stainless steel forgings have not been postweld heat treated in accordance with Table 4, the letters “WNS” shall be marked following the specification designation.
19.1.3 When test reports are required, the markings shall consist of the manufacturer’s symbol or name, the grade symbol, and such other markings as necessary to identify the part with the test report (19.1.1 and 19.1.2 shall apply).
19.1.4 Parts meeting all requirements for more than one class or grade may be marked with more than one class or grade designation such as F 304/F 304H, F 304/F 304L, and the like.
19.2 Bar Coding—In addition to the requirements in 19.1, bar coding is acceptable as a supplemental identification method. The purchaser may specify in the order a specific bar coding system to be used. The bar coding system, if applied at the discretion of the supplier, should be consistent with one of the published industry standards for bar coding. If used on small parts, the bar code may be applied to the box or a substantially applied tag.
20 Keywords
20.1 austenitic stainless steel; chromium alloy steel; chromium-molybdenum steel; ferritic/austenitic stainless steel; ferritic stainless steel; martensitic stainless steel; nickel alloy steel; notch toughness requirements; pipe fittings; piping applications; pressure containing parts; stainless steel fittings; stainless steel forgings; steel; steel flanges; steel forgings, alloy; steel valves; temperature service applications, elevated; temperature service applications, high; wrought material
SUPPLEMENTARY REQUIREMENTS
In addition to any of the supplementary requirements of Specification A961/A961M, the following supplementary requirements shall apply only when specified by the purchaser in the order.
S1. Macroetch Test
S1.1 A sample forging shall be sectioned and etched to show flow lines and internal imperfections. The test shall be conducted according to Test Method E340. Details of the test shall be agreed upon between the manufacturer and the purchaser.
S2. Heat Treatment Details
S2.1 The manufacturer shall furnish a detailed test report containing the information required in 18.2 and shall include all pertinent details of the heat-treating cycle given the forgings.
S3. Material for Optimum Resistance to Stress-Corrosion Cracking
S3.1 Austenitic stainless steel shall be furnished in the solution-annealed condition as a final operation with no subsequent cold working permitted, except, unless specifically prohibited by the purchaser, straightening of bars from which parts are machined is permitted to meet the requirements of Specification A484/A484M.
S4. Corrosion Tests
S4.1 All austenitic stainless steels shall pass intergranular corrosion tests performed in accordance with Practice E of Practices A262.
S4.2 Intergranular corrosion tests shall be performed on specimens of ferritic stainless steels as described in Practices A763.
S4.3 For both the austenitic and ferritic stainless steels, details concerning the number of specimens and their source and location are to be a matter of agreement between the manufacturer and the purchaser.
S5. Special Filler Metal
S5.1 In repair-welded F 316, F 316L, F 316H, and F 316N forgings, the deposited weld metal shall conform to E 308
composition wire. Forgings repair welded with E 308 weld metal shall be marked F __ W 308.
S6. Hardness Test
S6.1 Each forging shall be hardness tested and shall meet the requirements of Table 3.
S8. Heat Treatment of Austenitic Forgings
S8.1 The purchaser shall specify the heat-treatment method (in 7.1 or in 7.3.1) that shall be employed.
S8.2 The manufacturer shall provide a test report containing the information required in 18.2 and shall include a statement of the heat-treatment method employed.
S9. Grain Size for Austenitic Grades
S9.1 Forgings made from austenitic grades other than H grades shall be tested for average grain size by Test Method E112. Details of the test shall be agreed upon between the manufacturer and the purchaser.
S10. Stabilization Treatment
S10.1 Subsequent to the solution anneal for Grades F 321, F 321H, F 347, F 347H, F 348, and F 348H, these grades shall be given a stabilization heat treatment at 1500 to 1600 °F [815 to 870 °C] for a minimum of 2 h/in. [4.7 min/mm] of thickness and then cooling in the furnace or in air. In addition to the marking required in Section 19, the grade designation symbol shall be followed by the symbol “S10.”
S11. Grain Size Requirements for Non-H-Grade Austenitic Steels Used Above 1000 °F [540 °C]
S11.1 Non-H grades of austenitic stainless steels shall have a grain size of No. 7 or coarser as determined in accordance with Test Methods E112. The grain size so determined shall be on a certified test report.
Committee A01 has identified the location of selected changes to this specification since the last issue, A182/A182M–10a, that may impact the use of this specification. (Approved June 1, 2011)
(1) Added reference to Practice A388/A388M in 13.1 and Referenced Documents.
(2) Revised 7.2.1 and added 7.2.3 to permit Q&T of F 91 forgings having a section thickness greater than 3 in [75 mm] at the time of heat treatment and at the manufacturer’s option.
(3) Revised the minimum specified tensile strength and added
a minimum hardness for Grade F 91 in Table 3.
(4) Added new Section 13 on Nondestructive Test Requirements.
(5) Editorially revised Note C for F 24 in Table 4.
(6) Deleted Supplementary Requirement S7 from the specification.
Committee A01 has identified the location of selected changes to this specification since the last issue, A182/A182M–10, that may impact the use of this specification. (Approved November 1, 2010)
(1) Added Grade F347LN to Tables 1-4.
(2) Added ellipses (...) in Table 2 and revised Footnote A to explain them.
(3) Added HBW to column heading for Brinell Hardness Number in Table 3.
Committee A01 has identified the location of selected changes to this specification since the last issue, A182/A182M–09a, that may impact the use of this specification. (Approved May 1, 2010)
(1) Added reference to Specification A1049/A1049M in 1.3 and Referenced Documents.
(2) Revised 7.2 to clarify that when multiple heat treatment options are listed in Table 1, only one of the options need be exercised.
(3) Added reference to Test Method E92 in 9.6.3 and Referenced Documents.
(4) Added new Section 3 Terminology, including a definition for hardened condition, and renumbered subesquent sections.
(5) Revised chemistry requirements for F 23 in Table 2.
(6) Revised Table 2 to include ellipses where values are presently blank and to explain the meaning of the ellipses.
(7) Added new Footnote A to Table 3 explaining the meaning of the ellipses in the table.
(8) Added 2.4 to reference only AWS consumable material specifications rather than ASME SFA specifications. Also added A5.14/A5.14M, which was already referenced in Note G of Table 4; and added references to A5.23/A5.23M, A5.28/
A5.28M, and A5.29/A5.29M, new references for Grade F 91.
(9) Corrected reference to Supplementary Requirement S9 of Specification A961/A961M to S58 in 13.1.
(10) Changed references to ASME SFA specifications to AWS specifications and added A5.14/A5.14M, A5.23/A5.23M, A5.28/A5.28M, and A5.29/A5.29M in 13.1.2
(11) Revised Table 4 to change requirements for electrodes for F 91, F 92, F 911, and F 122, and changed references to ASME SFA specifications to AWS specifications.
(12) Revised Table 4 to revise electrodes listed for Grades F 5, F 5a, and F 9, since the previously listed AWS classifications A502 and A505 have been discontinued; and to add A5.14/ A5.14M, A5.23/A5.23M, and A5.28/A5.28M to Note A.
(13) Added Note F to the electrode designations for the H-grades of austenitic stainless steel forgings listed in Table 4. Added listings for H-grade electrodes where such AWS classifications exist.
This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years and if not revised, either reapproved or withdrawn. Your comments are invited either for revision of this standard or for additional standards and should be addressed to ASTM International Headquarters. Your comments will receive careful consideration at a meeting of the responsible technical committee, which you may attend. If you feel that your comments have not received a fair hearing you should make your views known to the ASTM Committee on Standards, at the address shown below.