ASTM A182 A182M-11a Standard Specification for Forged or Rolled Alloy and Stainless Steel Pipe Flang

文档天下 国外标准评论1阅读模式

1 Scope*

1.1 This specification
2 covers forged low alloy and stainless steel piping components for use in pressure systems. Included are flanges, fittings, valves, and similar parts to specified dimensions or to dimensional standards, such as the ASME specifications that are referenced in Section 2.

1.2 For bars and products machined directly from bar (other than those directly addressed by this specification; see 6.4), refer to Specifications A479/A479M and A739 for the similar grades available in those specifications. Products made to this specification are limited to a maximum weight of 10 000 lb [4540 kg]. For larger products and products for other applications, refer to Specifications A336/A336M and A965/A965M for the similar ferritic and austenitic grades, respectively, available in those specifications.

1.3 Several grades of low alloy steels and ferritic, martensitic, austenitic, and ferritic-austenitic stainless steels are included in this specification. Selection will depend upon design and service requirements. Several of the ferritic/austenitic (duplex) grades are also found in Specification A1049/ A1049M.

1.4 Supplementary requirements are provided for use when additional testing or inspection is desired. These shall apply only when specified individually by the purchaser in the order.

1.5 This specification is expressed in both inch-pound units and in SI units. However, unless the order specifies the applicable “M” specification designation (SI units), the material shall be furnished to inch-pound units.

1.6 The values stated in either SI units or inch-pound units are to be regarded separately as the standard. Within the text, the SI units are shown in brackets. The values stated in each

system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in non-conformance with the standard.

2 Referenced Documents

2.1 In addition to the referenced documents listed in Specification A961/A961M, the following list of standards apply to this specification.

2.2 ASTM Standards:
3

A262 Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels

A275/A275M Practice for Magnetic Particle Examination of Steel Forgings

A336/A336M Specification for Alloy Steel Forgings for Pressure and High-Temperature Parts

A388/A388M Practice for Ultrasonic Examination of Steel Forgings

A479/A479M Specification for Stainless Steel Bars and Shapes for Use in Boilers and Other Pressure Vessels

A484/A484M Specification for General Requirements for Stainless Steel Bars, Billets, and Forgings

A739 Specification for Steel Bars, Alloy, Hot-Wrought, for Elevated Temperature or Pressure-Containing Parts, or Both

A763 Practices for Detecting Susceptibility to Intergranular Attack in Ferritic Stainless Steels

A788/A788M Specification for Steel Forgings, General Requirements

A961/A961M Specification for Common Requirements for Steel Flanges, Forged Fittings, Valves, and Parts for Piping Applications

A965/A965M Specification for Steel Forgings, Austenitic, for Pressure and High Temperature Parts

A1049/A1049M Specification for Stainless Steel Forgings,

1 This specification is under the jurisdiction of ASTM Committee A01 on Steel, Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee A01.22 on Steel Forgings and Wrought Fittings for Piping Applications and Bolting Materials for Piping and Special Purpose Applications.

Current edition approved Oct. 1, 2011. Published November 2011. Originally approved in 1935. Last previous edition approved in 2011 as A182/A182M–11. DOI: 10.1520/A0182_A0182M-11a.

2 For ASME Boiler and Pressure Vessel Code applications see related Specification SA-182 in Section II of that Code.

3 For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards volume information, refer to the standard’s Document Summary page on the ASTM website.

Ferritic/Austenitic (Duplex), for Pressure Vessels and Re
lated Components

E92 Test Method for Vickers Hardness of Metallic Materials
4

E112 Test Methods for Determining Average Grain Size

E165 Practice for Liquid Penetrant Examination for General Industry

E340 Test Method for Macroetching Metals and Alloys

2.3 ASME Boiler and Pressure Vessel Codes:
5

Section IX Welding and Brazing Qualifications

2.4 AWS Specifications
6

A5.4/A5.4M Specification for Stainless Steel Electrodes for Shielded Metal Arc Welding

A5.5/A5.5M Specification for Low-Alloy Steel Electrodes for Shielded Metal Arc Welding

A5.9/A5.9M Specification for Bare Stainless Steel Welding Electrodes and Rods

A5.11/A5.11M Specification for Nickel and Nickel-Alloy Welding Electrodes for Shielded Metal Arc Welding

A5.14/A5.14M Specification for Nickel and Nickel-Alloy Bare Welding Electrodes and Rods

A5.23/A5.23M Specification for Low-Alloy Steel Electrodes and Fluxes for Submerged Arc Welding

A5.28/A5.28M Specification for Low-Alloy Steel Electrodes for Gas Shielded Arc Welding

A5.29/A5.29M Low-Alloy Steel Electrodes for Flux Cored Arc Welding

3 Terminology

3.1 Definitions—For definitions of terms used in this specification, refer to Specification A961/A961M.

3.2 Definitions of Terms Specific to This Standard:

3.2.1 hardened condition, n—for F23, the metallurgical condition achieved after normalizing and cooling to room temperature but prior to tempering.

4 Ordering Information

4.1 It is the purchaser’s responsibility to specify in the purchase order information necessary to purchase the needed material. In addition to the ordering information guidelines in Specification A961/A961M, orders should include the following information:

4.1.1 Additional requirements (see 7.2.1, Table 2 footnotes, 9.3, and 19.2), and

4.1.2 Requirement, if any, that manufacturer shall submit drawings for approval showing the shape of the rough forging before machining and the exact location of test specimen material (see 9.3.1).

5 General Requirements

5.1 Product furnished to this specification shall conform to the requirements of Specification A961/A961M, including any

supplementary requirements that are indicated in the purchase order. Failure to comply with the general requirements of Specification A961/A961M constitutes nonconformance with this specification. In case of conflict between the requirements of this specification and Specification A961/A961M, this specification shall prevail.

6 Manufacture

6.1 The low-alloy ferritic steels shall be made by the open-hearth, electric-furnace, or basic-oxygen process with the option of separate degassing and refining processes in each case.

6.2 The stainless steels shall be melted by one of the following processes: (a) electric-furnace (with the option of separate degassing and refining processes); (b) vacuumfurnace; or (c) one of the former followed by vacuum or electroslag-consumable remelting. Grade F XM-27Cb may be produced by electron-beam melting.

6.3 A sufficient discard shall be made to secure freedom from injurious piping and undue segregation.

6.4 The material shall be forged as close as practicable to the specified shape and size.

6.4.1 Flanges of any type, elbows, return bends, tees, and header tees shall not be machined directly from bar stock.

6.4.2 Cylindrically-shaped parts may be machined from forged or rolled solution-annealed austenitic stainless steel bar without additional hot working.

6.4.3 Small cylindrically-shaped low alloy and martensitic stainless steel parts, NPS-4 [DN 100] and under, may be machined from forged or rolled bar, without additional hot working.

6.5 Except as provided for in 6.4, the finished product shall be a forging as defined in the Terminology section of Specification A788/A788M.

7 Heat Treatment 7

7.1 After hot working, forgings shall be cooled to a temperature below 1000 °F [538 °C] prior to heat treating in accordance with the requirements of Table 1.

7.2 Low Alloy Steels and Ferritic and Martensitic Stainless Steels—The low alloy steels and ferritic and martensitic stainless steels shall be heat treated in accordance with the requirements of 7.1 and Table 1. When more than one heat treatment option is listed for a Grade in Table 1, any one of the heat treatments listed shall be performed. The selection of the heat treatment shall be at the manufacturer’s option, unless otherwise stated in the purchase order.

7.2.1 Liquid Quenching—Except as permitted in 7.2.2, for F 1, F 2, and F 3, and in 7.2.3, for F 91, and when agreed to by the purchaser, liquid quenching followed by tempering shall be permitted provided the temperatures in Table 1 for each grade are used.

4 Withdrawn. The last approved version of this historical standard is referenced on www.astm.org.

5 Available from American Society of Mechanical Engineers (ASME), ASME International Headquarters, Three Park Ave., New York, NY 10016-5990, http:// www.asme.org.

6 Available from American Welding Society (AWS), 550 NW LeJeune Rd., Miami, FL 33126, http://www.aws.org.

7 A solution annealing temperature above 1950 °F [1065 °C] may impair the resistance to intergranular corrosion after subsequent exposure to sensitizing conditions in F 321, F 321H, F 347, F 347H, F 348, and F 348H. When specified by the purchaser, a lower temperature stabilization or resolution annealing shall be used subsequent to the initial high temperature solution anneal (see Supplementary Requirement S10).

7.2.1.1 Marking—Parts that are liquid quenched and tempered shall be marked “QT.”

7.2.2 Alternatively, Grade F 1, F 2, and F 12, Classes 1 and 2 may be given a heat treatment of 1200 °F [650 °C] minimum after final hot or cold forming.

7.2.3 Alternatively, Grade F 91 forged fittings having any section thickness greater than 3 in. [75 mm], at the time of heat treatment, shall be normalized and tempered or quenched and tempered at the manufacturer’s option, provided that the temperatures in Table 1 for F 91 are used.

7.3 Austenitic and Ferritic-Austenitic Stainless Steels—The austenitic and ferritic-austenitic stainless steels shall be heat treated in accordance with the requirements of 7.1 and Table 1.

7.3.1 Alternatively, immediately following hot working, while the temperature of the forging is not less than the minimum solution annealing temperature specified in Table 1,

forgings made from austenitic grades (except grades F 304H, F 309H, F 310, F 310H, F 316H, F 321, F 321H, F 347, F 347H, F 348, F 348H, F 45, and F 56) may be individually rapidly quenched in accordance with the requirements of Table 1.

7.3.2 See Supplementary Requirement S8 if a particular heat treatment method is to be employed.

7.4 Time of Heat Treatment—Heat treatment of forgings may be performed before machining.

7.5 Forged or Rolled Bar—Forged or rolled austenitic stainless bar from which cylindrically shaped parts are to be machined, as permitted by 6.4, and the parts machined from such bar, without heat treatment after machining, shall be furnished to the annealing requirements of Specification A479/ A479M or this specification, with subsequent light cold drawing and straightening permitted (see Supplementary Requirement S3 if annealing must be the final operation).

TABLE 1 Heat Treating Requirements
Grade Heat Treat Type Austenitizing/Solutioning Temperature, Minimum or Range, °F [°C]A Cooling Media Quenching Cool Below °F [°C] Tempering Temperature, Minimum or Range, °F [°C]
Low Alloy Steels
F 1 anneal 1650 [900] furnace cool B B
normalize and temper 1650 [900] air cool B 1150 [620]
F 2 anneal 1650 [900] furnace cool B B
normalize and temper 1650 [900] air cool B 1150 [620]
F 5, F 5a anneal 1750 [955] furnace cool B B
normalize and temper 1750 [955] air cool B 1250 [675]
F 9 anneal 1750 [955] furnace cool B B
normalize and temper 1750 [955] air cool B 1250 [675]
F 10 solution treat and quench 1900 [1040] liquid 500 [260] B
F 91 normalize and temper 1900-1975 [1040-1080] air cool B 1350-1470 [730-800]
F 92 normalize and temper 1900-1975 [1040-1080] air cool B 1350-1470 [730-800]
F 122 normalize and temper 1900-1975 [1040-1080] air cool B 1350-1470 [730-800]
F 911 normalize and temper 1900-1975 [1040-1080] air cool or liquid B 1365-1435 [740-780]
F 11, Class 1, 2, 3 anneal 1650 [900] furnace cool B B
normalize and temper 1650 [900] air cool B 1150 [620]
F 12, Class 1, 2 anneal 1650 [900] furnace cool B B
normalize and temper 1650 [900] air cool B 1150 [620]
F 21, F 3V, and F 3VCb anneal 1750 [955] furnace cool B B
normalize and temper 1750 [955] air cool B 1250 [675]
F 22, Class 1, 3 anneal 1650 [900] furnace cool B B
normalize and temper 1650 [900] air cool B 1250 [675]
F 22V normalize and temper or quench and temper 1650 [900] air cool or liquid B 1250 [675]
F 23 normalize and temper 1900-1975 [1040-1080] air cool B 1350-1470 [730-800]
accelerated cool
F 24 normalize and temper 1800-1975 [980-1080] air cool or liquid B 1350-1470 [730-800]
FR anneal 1750 [955] furnace cool B B
normalize 1750 [955] air cool B B
normalize and temper 1750 [955] air cool B 1250 [675]
F 36, Class 1 normalize and temper 1650 [900] air cool B 1100 [595]
F 36, Class 2 normalize and temper 1650 [900] air cool B 1100 [595]
quench and temper 1650 [900] accelerated air cool or liquid 1100 [595]
Martensitic Stainless Steels
F 6a Class 1 anneal not specified furnace cool B B
normalize and temper not specified air cool 400 [205] 1325 [725]
temper not required B B 1325 [725]
F 6a Class 2 anneal not specified furnace cool B B
normalize and temper not specified air cool 400 [205] 1250 [675]
temper not required B B 1250 [675]
F 6a Class 3 anneal not specified furnace cool B B
normalize and temper not specified air cool 400 [205] 1100 [595]
F 6a Class 4 anneal not specified furnace cool B B
normalize and temper not specified air cool 400 [205] 1000 [540]
TABLE 1 Continued
Grade Heat Treat Type Austenitizing/Solutioning Temperature, Minimum or Range, °F [°C]A Cooling Media Quenching Cool Below °F [°C] Tempering Temperature, Minimum or Range, °F [°C]
F 6b anneal 1750 [955] furnace cool B B
normalize and temper 1750 [955] air cool 400 [205] 1150 [620]
F 6NM normalize and temper 1850 [1010] air cool 200 [95] 1040-1120 [560-600]
Ferritic Stainless Steels
F XM-27 Cb anneal 1850 [1010] furnace cool B B
F 429 anneal 1850 [1010] furnace cool B B
F 430 anneal not specified furnace cool B B
Austenitic Stainless Steels
F 304 solution treat and quench 1900 [1040] liquid 500 [260] B
F 304H solution treat and quench 1900 [1040] liquid 500 [260] B
F 304L solution treat and quench 1900 [1040] liquid 500 [260] B
F 304N solution treat and quench 1900 [1040] liquid 500 [260] B
F 304LN solution treat and quench 1900 [1040] liquid 500 [260] B
F 309H solution treat and quench 1900 [1040] liquid 500 [260] B
F 310 solution treat and quench 1900 [1040] liquid 500 [260] B
F 310H solution treat and quench 1900 [1040] liquid 500 [260] B
F 310MoLN solution treat and quench 1900-2010 [1050-1100] liquid 500 [260] B
F 316 solution treat and quench 1900 [1040] liquid 500 [260] B
F 316H solution treat and quench 1900 [1040] liquid 500 [260] B
F 316L solution treat and quench 1900 [1040] liquid 500 [260] B
F 316N solution treat and quench 1900 [1040] liquid 500 [260] B
F 316LN solution treat and quench 1900 [1040] liquid 500 [260] B
F 316Ti solution treat and quench 1900 [1040] liquid 500 [260] B
F 317 solution treat and quench 1900 [1040] liquid 500 [260] B
F 317L solution treat and quench 1900 [1040] liquid 500 [260] B
S31727 solution treat and quench 1975-2155 [1080-1180] liquid 500 [260] B
S32053 solution treat and quench 1975-2155 [1080-1180] liquid 500 [260] B
F 347 solution treat and quench 1900 [1040] liquid 500 [260] B
F 347H solution treat and quench 2000 [1095] liquid 500 [260] B
F 347LN solution treat and quench 1900 [1040] liquid 500 [260] B
F 348 solution treat and quench 1900 [1040] liquid 500 [260] B
F 348H solution treat and quench 2000 [1095] liquid 500 [260] B
F 321 solution treat and quench 1900 [1040] liquid 500 [260] B
F 321H solution treat and quench 2000 [1095] liquid 500 [260] B
F XM-11 solution treat and quench 1900 [1040] liquid 500 [260] B
F XM-19 solution treat and quench 1900 [1040] liquid 500 [260] B
F 20 solution treat and quench 1700-1850 [925-1010] liquid 500 [260] B
F 44 solution treat and quench 2100 [1150] liquid 500 [260] B
F 45 solution treat and quench 1900 [1040] liquid 500 [260] B
F 46 solution treat and quench 2010-2140 [1100-1140] liquid 500 [260] B
F 47 solution treat and quench 1900 [1040] liquid 500 [260] B
F 48 solution treat and quench 1900 [1040] liquid 500 [260] B
F 49 solution treat and quench 2050 [1120] liquid 500 [260] B
F 56 solution treat and quench 2050-2160 [1120-1180] liquid 500 [260] B
F 58 solution treat and quench 2085 [1140] liquid 500 [260] B
F 62 solution treat and quench 2025 [1105] liquid 500 [260] B
F 63 solution treat and quench 1900 [1040] liquid 500 [260] B
F 64 solution treat and quench 2010-2140 [1100-1170] liquid 500 [250] B
F 904L solution treat and quench 1920-2100 [1050-1150] liquid 500 [260] B
Ferritic-Austenitic Stainless Steels
F 50 solution treat and quench 1925 [1050] liquid 500 [260] B
F 51 solution treat and quench 1870 [1020] liquid 500 [260] B
F 52C liquid 500 [260] B
F 53 solution treat and quench 1880 [1025] liquid 500 [260] B
F 54 solution treat and quench 1920-2060 [1050-1125] liquid 500 [260] B
F 55 solution treat and quench 2010-2085 [1100-1140] liquid 500 [260] B
F 57 solution treat and quench 1940 [1060] liquid 175 [80] B
F 59 solution treat and quench 1975-2050 [1080-1120] liquid 500 [260] B
F 60 solution treat and quench 1870 [1020] liquid 500 [260] B
F 61 solution treat and quench 1920-2060 [1050-1125] liquid 500 [260] B
F 65 solution treat and quench 1830-2100 [1000-1150] liquidD 500 [260] B
F 66 solution treat and quench 1870-1975 [1020-1080] liquid 500 [260] B
F 67 solution treat and quench 1870-2050 [1020-1120] liquid 500 [260] B
A Minimum unless temperature range is listed.
B Not applicable.
C Grade F 52 shall be solution treated at 1825 to 1875 °F [995 to 1025 °C] 30 min/in. of thickness and water quenched.
D The cooling media for Grade F 65 shall be quenching in water or rapidly cooling by other means.

8 Chemical Composition

8.1 A chemical heat analysis in accordance with Specification A961/A961M shall be made and conform to the chemical composition prescribed in Table 2.

8.2 Grades to which lead, selenium, or other elements are added for the purpose of rendering the material free-machining shall not be used.

8.3 Starting material produced to a specification that specifically requires the addition of any element beyond those listed in Table 2 for the applicable grade of material is not permitted.

8.4 Steel grades covered in this specification shall not contain an unspecified element, other than nitrogen in stainless steels, for the ordered grade to the extent that the steel conforms to the requirements of another grade for which that element is a specified element having a required minimum content. For this requirement, a grade is defined as an alloy described individually and identified by its own UNS designation or Grade designation and identification symbol in Table 2.

8.5 Product Analysis—The purchaser may make a product analysis on products supplied to this specification in accordance with Specification A961/A961M.

9 Mechanical Properties

9.1 The material shall conform to the requirements as to mechanical properties for the grade ordered as listed in Table 3.

9.2 Mechanical test specimens shall be obtained from production forgings, or from separately forged test blanks pre-pared from the stock used to make the finished product. In either case, mechanical test specimens shall not be removed until after all heat treatment is complete. If repair welding is required, test specimens shall not be removed until after post-weld heat treatment is complete, except for ferritic grades when the post-weld heat treatment is conducted at least 50 °F [30 °C] below the actual tempering temperature. When test blanks are used, they shall receive approximately the same working as the finished product. The test blanks shall be heat treated with the finished product and shall approximate the maximum cross section of the forgings they represent.

9.3 For normalized and tempered, or quenched and tempered forgings, the central axis of the test specimen shall correspond to the 1⁄4 T plane or deeper position where T is the maximum heat-treated thickness of the represented forging. In addition, for quenched and tempered forgings, the mid-length of the test specimen shall be at least T from any second heat-treated surface. When the section thickness does not permit this positioning, the test specimen shall be positioned as near as possible to the prescribed location, as agreed to by the purchaser and the supplier.

9.3.1 With prior purchase approval, the test specimen for ferritic steel forgings may be taken at a depth (t) corresponding to the distance from the area of significant stress to the nearest heat-treated surface and at least twice this distance (2 t) from any second surface. However, the test depth shall not be nearer to one treated surface than 3⁄4 in. [19 mm] and to the second treated surface than 1
1
⁄2 in. [38 mm]. This method of test specimen location would normally apply to contour-forged parts, or parts with thick cross-sectional areas where 1⁄4 T 3

T testing (see 9.3) is not practical. Sketches showing the exact test locations shall be approved by the purchaser when this method is used.

9.3.2 Metal Buffers—The required distances from heattreated surfaces may be obtained with metal buffers instead of integral extensions. Buffer material may be carbon or low-alloy steel, and shall be joined to the forging with a partial penetration weld that seals the buffered surface. Specimens shall be located at 1
⁄2-in. [13-mm] minimum from the buffered surface of the forging. Buffers shall be removed and the welded areas subjected to magnetic particle test to ensure freedom from cracks unless the welded areas are completely removed by subsequent machining.

9.4 For annealed low alloy steels, ferritic stainless steels, and martensitic stainless steels, and also for austenitic and ferritic-austenitic stainless steels, the test specimen may be taken from any convenient location.

9.5 Tension Tests:

9.5.1 Low Alloy Steels and Ferritic and Martensitic Stainless Steels—One tension test shall be made for each heat in each heat treatment charge.

9.5.1.1 When the heat-treating cycles are the same and the furnaces (either batch or continuous type) are controlled within ±25°F [(±14°C)] and equipped with recording pyrometers so that complete records of heat treatment are available, then only one tension test from each heat of each forging type (see Note 1) and section size is required, instead of one test from each heat in each heat-treatment charge. NOTE 1—“Type” in this case is used to describe the forging shape such as a flange, ell, tee, and the like.

9.5.2 Austenitic and Ferritic-Austenitic Stainless Steel Grades—One tension test shall be made for each heat.

9.5.2.1 When heat treated in accordance with 7.1, the test blank or forging used to provide the test specimen shall be heat treated with a finished forged product.

9.5.2.2 When the alternative method in 7.3.1 is used, the test blank or forging used to provide the test specimen shall be forged and quenched under the same processing conditions as the forgings they represent.

9.5.3 Testing shall be performed as specified in Specification A961/A961M using the largest feasible of the round specimens.

9.6 Hardness Tests:

9.6.1 Except when only one forging is produced, a minimum of two pieces per batch or continuous run as defined in 9.6.2 shall be hardness tested as specified in Specification A961/A961M to ensure that the forgings are within the hardness limits given for each grade in Table 3. The purchaser may verify that the requirement has been met by testing at any location on the forging provided such testing does not render the forging useless.

9.6.2 When the reduced number of tension tests permitted by 9.5.1.1 is applied, additional hardness tests shall be made on forgings or samples, as defined in 9.2, scattered throughout the load (see Note 2). At least eight samples shall be checked from each batch load, and at least one check per hour shall be made from a continuous run. When the furnace batch is less than eight forgings, each forging shall be checked. If any check falls

outside the prescribed limits, the entire lot of forgings shall be reheat treated and the requirements of 9.5.1 shall apply. NOTE 2—The tension test required in 9.5.1 is used to determine material capability and conformance in addition to verifying the adequacy of the heat-treatment cycle. Additional hardness tests in accordance with 9.6.2 are required when 9.5.1.1 is applied to ensure the prescribed heat-treating cycle and uniformity throughout the load.

9.6.3 When the alternative to the Ti/N ratio limit for F23 is applied, (see Note P in Table 2), a minimum of two pieces per batch or continuous run as defined in 9.6.2 shall be hardness tested, in the hardened condition (see 3.2.1), to ensure that the

forgings are within the hardness limit given for F23 in Note P of Table 2. The test samples shall be taken at the mid thickness of the thickest section of the product. Testing shall be performed in accordance with the Test Method E92 or as specified in Specification A961/A961M.

9.7 Notch Toughness Requirements—Grades F 3V, F 3VCb, and F 22V.

9.7.1 Impact test specimens shall be Charpy V-notch Type. The usage of subsize specimens due to material limitations must have prior purchaser approval.

TAB LE 2 Chem ical Req u i rements A
Identification Symbol UNS Designation Grade Composition, %
Carbon Manganese Phosphorus Sulfur Silicon Nickel Chromium Molybdenum Columbium Titanium Other Elements
Low Alloy Steels
F 1 K12822 carbon-molybdenum 0.28 0.60–0.90 0.045 0.045 0.15–0.35 ... ... 0.44–0.65 ... ... ...
F 2B K12122 0.5 % chromium, 0.5 % molybdenum 0.05–0.21 0.30–0.80 0.040 0.040 0.10–0.60 ... 0.50–0.81 0.44–0.65 ... ... ...
F 5C K41545 4 to 6 % chromium 0.15 0.30–0.60 0.030 0.030 0.50 0.50 4.0–6.0 0.44–0.65 ... ... ...
F 5aC K42544 4 to 6 % chromium 0.25 0.60 0.040 0.030 0.50 0.50 4.0–6.0 0.44–0.65 ... ... ...
F 9 K90941 9 % chromium 0.15 0.30–0.60 0.030 0.030 0.50–1.00 ... 8.0–10.0 0.90–1.10 ... ... ...
F 10 S33100 20 nickel, 8 chromium 0.10–0.20 0.50–0.80 0.040 0.030 1.00–1.40 19.0–22.0 7.0–9.0 ... ... ... ...
F 91 K90901 9 % chromium, 1 % molybdenum, 0.2 % vanadium plus columbium and nitrogen 0.08–0.12 0.30–0.60 0.020 0.010 0.20–0.50 0.40 8.0–9.5 0.85–1.05 0.06–0.10 ... N 0.03–0.07Al 0.02DV 0.18–0.25Ti 0.01DZr 0.01D
F 92 K92460 9 % chromium, 1.8 % tungsten, 0.2 % vanadium plus columbium 0.07–0.13 0.30–0.60 0.020 0.010 0.50 0.40 8.50–9.50 0.30–0.60 0.04–0.09 ... V 0.15–0.25N0.030–0.070Al 0.02DW 1.50–2.00B0.001–0.006Ti 0.01DZr 0.01D
F 122 K91271 11 % chromium, 2 % tungsten, 0.2 % vanadium, plus molybdenum, columbium, copper, nickel, nitrogen, and boron 0.07–0.14 0.70 0.020 0.010 0.50 0.50 10.00–11.50 0.25–0.60 0.04–0.10 ... V 0.15–0.30B 0.005N 0.040–0.100Al 0.02DCu 0.30–1.70W 1.50–2.50Ti 0.01DZr 0.01D
F 911 K91061 9 % chromium, 1 % molybdenum, 0.2 % vanadium plus columbium and nitrogen 0.09–0.13 0.30–0.60 0.020 0.010 0.10–0.50 0.40 8.5–9.5 0.90–1.10 0.060–0.10 ... W 0.90–1.10Al 0.02DN 0.04–0.09V 0.18–0.25B 0.0003–0.006Ti 0.01DZr 0.01D
F 11Class 1 K11597 1.25 % chromium, 0.5 % molybdenum 0.05–0.15 0.30–0.60 0.030 0.030 0.50–1.00 ... 1.00–1.50 0.44–0.65 ... ... ...
F 11Class 2 K11572 1.25 % chromium, 0.5 % molybdenum 0.10–0.20 0.30–0.80 0.040 0.040 0.50–1.00 ... 1.00–1.50 0.44–0.65 ... ... ...
F 11Class 3 K11572 1.25 % chromium, 0.5 % molybdenum 0.10–0.20 0.30–0.80 0.040 0.040 0.50–1.00 ... 1.00–1.50 0.44–0.65 ... ... ...
F 12Class 1 K11562 1 % chromium, 0.5 % molybdenum 0.05–0.15 0.30–0.60 0.045 0.045 0.50 max ... 0.80–1.25 0.44–0.65 ... ... ...
F 12Class 2 K11564 1 % chromium, 0.5 % molybdenum 0.10–0.20 0.30–0.80 0.040 0.040 0.10–0.60 ... 0.80–1.25 0.44–0.65 ... ... ...
F 21 K31545 chromium-molybdenum 0.05–0.15 0.30–0.60 0.040 0.040 0.50 max ... 2.7–3.3 0.80–1.06 ... ... ...

A182/A182M - 11a

TABLE 2 Continued
Identification Symbol UNS Designation Grade Composition, %
Carbon Manganese Phosphorus Sulfur Silicon Nickel Chromium Molybdenum Columbium Titanium Other Elements
F 3V K31830 3 % chromium, 1 % molybdenum, 0.25 % vanadium plus boron and titanium 0.05–0.18 0.30–0.60 0.020 0.020 0.10 ... 2.8–3.2 0.90–1.10 ... 0.015–0.035 V 0.20–0.30 B 0.001–0.003
F 3VCb K31390 3 % chromium, 1 % molybdenum, 0.25 % vanadium plus boron, columbium, and titanium 0.10–0.15 0.30–0.60 0.020 0.010 0.10 0.25 2.7–3.3 0.90–1.10 0.015–0.070 0.015 V 0.20–0.30 Cu 0.25 Ca 0.0005–0.0150
F 22 Class 1 K21590 chromium-molybdenum 0.05–0.15 0.30–0.60 0.040 0.040 0.50 ... 2.00–2.50 0.87–1.13 ... ... ...
F 22 Class 3 K21590 chromium-molybdenum 0.05–0.15 0.30–0.60 0.040 0.040 0.50 ... 2.00–2.50 0.87–1.13 ... ... ...
F 22V K31835 2.25 % chromium, 1 % molybdenum, 0.25 % vanadium 0.11–0.15 0.30–0.60 0.015 0.010 0.10 0.25 2.00–2.50 0.90–1.10 0.07 0.030 Cu 0.20 V 0.25–0.35 B 0.002 Ca 0.015E
F 23 K41650 2.25 % chromium, 1.6 % tungsten, 0.25 % vanadium, plus molybdenum, columbium, and boron 0.04–0.10 0.10–0.60 0.030 0.010 0.50 0.40 1.90–2.60 0.05–0.30 0.02–0.08 0.005–0.060F V 0.20–0.30 B 0.0010–0.006 N 0.015F Al 0.030 W 1.45–1.75
F 24 K30736 2.25 % chromium, 1 % molybdenum, 0.25 % vanadium plus titanium and boron 0.05–0.10 0.30–0.70 0.020 0.010 0.15–0.45 ... 2.20–2.60 0.90–1.10 ... 0.06–0.10 V 0.20–0.30 N 0.12 Al 0.020 B 0.0015–0.0070
FR K22035 2 % nickel, 1 % copper 0.20 0.40–1.06 0.045 0.050 ... 1.60–2.24 ... ... ... ... Cu 0.75–1.25 N 0.020 Al 0.050 Cu 0.50–0.80 V 0.02
F 36 K21001 1.15 % nickel, 0.65 % copper, molybdenum, and columbium 0.10–0.17 0.80–1.20 0.030 0.025 0.25–0.50 1.00–1.30 0.30 0.25–0.50 0.015–0.045 ... ...
Martensitic Stainless Steels
F 6a S41000 13 % chromium 410G 0.15 1.00 0.040 0.030 1.00 0.50 11.5–13.5 ... ... ... ...
F 6b S41026 13 % chromium, 0.5 % molybdenum 0.15 1.00 0.020 0.020 1.00 1.00–2.00 11.5–13.5 0.40–0.60 ... ... Cu 0.50
F 6NM S41500 13 % chromium, 4 % nickel 0.05 0.50–1.00 0.030 0.030 0.60 3.5–5.5 11.5–14.0 0.50–1.00 ... ... ...
Ferritic Stainless Steels
F XM-27CbH S44627 27 chromium, 1 molybdenum XM-27G 0.010 0.40 0.020 0.020 0.40 0.50 25.0–27.5 0.75–1.50 0.05–0.20 N 0.015 Cu 0.20
F 429 S42900 15 chromium 429G 0.12 1.00 0.040 0.030 0.75 0.50 14.0–16.0 ... ... ... ...
F 430 S43000 17 chromium 430G 0.12 1.00 0.040 0.030 0.75 0.50 16.0–18.0 ... ... ... ...
Austenitic Stainless Steels
F 304I S30400 18 chromium, 8 nickel 304G 0.08 2.00 0.045 0.030 1.00 8.0–11.0 18.0–20.0 ... ... ... ...

A182/A182M-11a

TABLE 2 Continued
Grade Composition, %
Carbon Manganese Phosphorus Sulfur Silicon Nickel Chromium Molybdenum Columbium Titanium Other Elements
18 chromium, 8 nickel 304HG 0.04–0.10 2.00 0.045 0.030 1.00 8.0–11.0 18.0–20.0 ... ... ... ...
18 chromium, 8 nickel, low carbon 304LG 0.030 2.00 0.045 0.030 1.00 8.0–13.0 18.0–20.0 ... ... ... ...
18 chromium, 8 nickel, modified with nitrogen 304NG 0.08 2.00 0.045 0.030 1.00 8.0–10.5 18.0–20.0 ... ... ... ...
18 chromium, 8 nickel, modified with nitrogen 304LNG 0.030 2.00 0.045 0.030 1.00 8.0–10.5 18.0–20.0 ... ... ... ...
23 chromium, 13.5 nickel 309HG 0.04–0.10 2.00 0.045 0.030 1.00 12.0–15.0 22.0–24.0 ... ... ... ...
25 chromium, 20 nickel 310G 0.25 2.00 0.045 0.030 1.00 19.0–22.0 24.0–26.0 ... ... ... ...
25 chromium, 20 nickel 310HG 0.04–0.10 2.00 0.045 0.030 1.00 19.0–22.0 24.0–26.0 ... ... ... ...
25 chromium, 22 nickel, modified with molybdenum and nitrogen, low carbon 310MolNG 0.030 2.00 0.030 0.015 0.40 21.0–23.0 24.0–26.0 2.00–3.00 ... ... N 0.10–0.16
18 chromium, 8 nickel, modified with molybdenum 316G 0.08 2.00 0.045 0.030 1.00 10.0–14.0 16.0–18.0 2.00–3.00 ... ... ...
18 chromium, 8 nickel, modified with molybdenum 316HG 0.04–0.10 2.00 0.045 0.030 1.00 10.0–14.0 16.0–18.0 2.00–3.00 ... ... ...
18 chromium, 8 nickel, modified with molybdenum, low carbon 316LG 0.030 2.00 0.045 0.030 1.00 10.0–15.0 16.0–18.0 2.00–3.00 ... ... ...
18 chromium, 8 nickel, modified with molybdenum and nitrogen 316NG 0.08 2.00 0.045 0.030 1.00 11.0–14.0 16.0–18.0 2.00–3.00 ... ... ...
18 chromium, 8 nickel, modified with molybdenum and nitrogen 316LNG 0.030 2.00 0.045 0.030 1.00 11.0–14.0 16.0–18.0 2.00–3.00 ... ... ...
18 chromium, 8 nickel, modified with molybdenum and nitrogen 316Ti 0.08 2.00 0.045 0.030 1.00 10.0–14.0 16.0–18.0 2.00–3.00 ... K N 0.10 max
19 chromium, 13 nickel, 3.5 molybdenum 317G 0.08 2.00 0.045 0.030 1.00 11.0–15.0 18.0–20.0 3.0–4.0 ... ... ...

A182/A182M - 11a

Identifi-cation Symbol U NS Desig-nation G rade
F 31 7L S31 703 1 9 ch romium , 1 3 nickel , 3.5 molybdenum 31 7LG
S31 727 S31 727 1 8 ch romium , 1 5 nickel , 4.5 molybdenum , 3.5 copper with nitrogen
S32053 S32053 23 ch romium , 25 nickel , 5.5 molybdenum , with nitrogen
F 32 1 S32 1 00 1 8 ch romium , 8 nickel modified with titanium 32 1 G
F 32 1 H S32 1 09 1 8 ch romium , 8 nickel , modified with titanium 32 1 H G
F 347 S34700 1 8 ch romium , 8 nickel modified with columbium347G
F 347H S34709 1 8 ch romium , 8 nickel , modified with columbium 347H G
F347LN S3475 1 1 8 ch romium , 8 nickel modified with columbium and nitrogen347LN
F 348 S34800 1 8 ch romium , 8 nickel modified with columbium348G
F 348H S34809 1 8 ch romium , 8 nickel , modified with columbium 348H G
F XM- 1 1 S2 1 904 20 ch romium , 6 nickel , 9 manganese XM- 1 1 G
F XM- 1 9 S209 1 0 22 ch romium , 1 3 nickel , 5 manganese XM- 1 9G
F 20 N08020 35 nickel , 20 ch romium , 3.5 copper, 2.5 molybdenum
F 44 S31 254 20 ch romium , 1 8 nickel , 6 molybdenum , low carbon
F 45 S3081 5 2 1 ch romium , 1 1 nickel modified with nitrogen and cerium
TABLE 2 Continued
Com position , %
Carbon Manga-nese Phos-phorus Sulfu r Silicon N ickel Ch romium Molybde-num Colum-bium Titan-ium Other Elements
0.030 2.00 0.045 0.030 1 .00 1 1 .0-1 5.0 1 8.0-20.0 3.0-4.0 . . . . . . . . .
0.030 1 .00 0.030 0.030 1 .00 1 4.5-1 6.5 1 7.5-1 9.0 3.8-4.5 . . . . . . Cu 2.8-4.0 N 0. 1 5-0.2 1
0.030 1 .00 0.030 0.01 0 1 .00 24.0-28.0 22.0-24.0 5.0-6.0 . . . . . . N 0. 1 7-0.22
0.08 2.00 0.045 0.030 1 .00 9.0-1 2.0 1 7.0-1 9.0 . . . . . . L . . .
0.04-0. 1 0 2.00 0.045 0.030 1 .00 9.0-1 2.0 1 7.0-1 9.0 . . . . . . M . . .
0.08 2.00 0.045 0.030 1 .00 9.0-1 3.0 1 7.0-20.0 . . . N . . . . . .
0.04-0. 1 0 2.00 0.045 0.030 1 .00 9.0-1 3.0 1 7.0-20.0 . . . O . . . . . .
0.005-0.020 2.00 0.045 0.030 1 .00 9.0-1 3.0 1 7.0-1 9.0 . . . 0.20-0.50P . . . N 0.06-0. 1 0
0.08 2.00 0.045 0.030 1 .00 9.0-1 3.0 1 7.0-20.0 . . . N . . . Co 0.20 Ta 0. 1 0
0.04-0. 1 0 2.00 0.045 0.030 1 .00 9.0-1 3.0 1 7.0-20.0 . . . O . . . Co 0.20 Ta 0. 1 0
0.040 8.0-1 0.0 0.060 0.030 1 .00 5.5-7.5 1 9.0-2 1 .5 . . . . . . . . . N 0. 1 5-0.40
0.06 4.0-6.0 0.040 0.030 1 .00 1 1 .5-1 3.5 20.5-23.5 1 .50-3.00 0. 1 0-0.30 . . . N 0.20-0.40 V 0. 1 0-0.30
.07 2.00 0.045 0.035 1 .00 32.0-38.0 1 9.0-2 1 .0 2.00-3.00 8xCmin-1 .00 . . . Cu 3.0-4.0
0.020 1 .00 0.030 0.01 0 0.80 1 7.5-1 8.5 1 9.5-20.5 6.0-6.5 . . . . . . Cu 0.50-1 .00 N 0. 1 8-0.22
0.05-0. 1 0 0.80 0.040 0.030 1 .40-2.00 1 0.0-1 2.0 20.0-22.0 . . . . . . . . . N 0. 1 4-0.20 Ce 0.03-0.08

A182/A182M - 11a

Identifi-cation Symbol U NS Desig-nation G rade
F 46 S30600 1 8 ch romium , 1 5 nickel , 4 silicon
F 47 S31 725 1 9 ch romium , 1 5 nickel , 4 molybdenum 31 7LMG
F 48 S31 726 1 9 ch romium , 1 5 nickel , 4 molybdenum 31 7LM N G
F 49 S34565 24 ch romium , 1 7 nickel , 6 manganese, 5 molybdenum
F 56 S33228 32 nickel , 27 ch romium with columbium
F 58 S31 266 24 ch romium , 20 nickel , 6 molybdenum , 2 tungsten with nitrogen
F 62 N08367 2 1 ch romium , 25 nickel , 6.5 molybdenum
F 63 S3261 5 1 8 ch romium , 20 nickel , 5.5 silicon
F 64 S30601 1 7.5 ch romium , 1 7.5 nickel , 5.3 silicon
F 904L N08904 2 1 ch romium , 26 nickel , 4.5 molybdenum 904LG
TABLE 2 Continued
Composition, %
Carbon Manganese Phosphorus Sulfur Silicon Nickel Chromium Molybdenum Columbium Titanium Other Elements
0.018 2.00 0.020 0.020 3.7–4.3 14.0–15.5 17.0–18.5 0.20 ... ... Cu 0.50
0.030 2.00 0.045 0.030 0.75 13.0–17.5 18.0–20.0 4.0–5.0 ... ... N 0.10
0.030 2.00 0.045 0.030 0.75 13.5–17.5 17.0–20.0 4.0–5.0 ... ... N 0.10–0.20
0.030 5.0–7.0 0.030 0.010 1.00 16.0–18.0 23.0–25.0 4.0–5.0 0.10 ... N 0.40–0.60
0.04–0.08 1.00 0.020 0.015 0.30 31.0–33.0 26.0–28.0 ... 0.6–1.0 ... Ce 0.05–0.10Al 0.025
0.030 2.0–4.0 0.035 0.020 1.00 21.0–24.0 23.0–25.0 5.2–6.2 ... ... N 0.35–0.60Cu 1.00–2.50W 1.50–2.50
0.030 2.00 0.040 0.030 1.00 23.5–25.5 20.0–22.0 6.0–7.0 ... ... N 0.18–0.25Cu 0.75
0.07 2.00 0.045 0.030 4.8-6.0 19.0-22.0 16.5-19.5 0.30-1.50 ... ... Cu 1.50-2.50
0.015 0.50-0.80 0.030 0.013 5.0-5.6 17.0-18.0 17.0-18.0 0.20 ... ... Cu 0.35, N 0.05
0.020 2.0 0.040 0.030 1.00 23.0–28.0 19.0–23.0 4.0–5.0 ... ... Cu 1.00–2.00N 0.10
Ferritic-Austenitic Stainless Steels
F 50 S31200 25 chromium, 6 nickel, modified with nitrogen 0.030 2.00 0.045 0.030 1.00 5.5–6.5 24.0–26.0 1.20–2.00 ... ... N 0.14–0.20
F 51 S31803 22 chromium, 5.5 nickel, modified with nitrogen 0.030 2.00 0.030 0.020 1.00 4.5–6.5 21.0–23.0 2.5–3.5 ... ... N 0.08–0.20
F 52 S32950 26 chromium, 3.5 nickel, 1.0 molybdenum 0.030 2.00 0.035 0.010 0.60 3.5–5.2 26.0–29.0 1.00–2.50 ... ... N 0.15–0.35
F 53 S32750 25 chromium, 7 nickel, 4 molybdenum, modified with nitrogen 2507G 0.030 1.20 0.035 0.020 0.80 6.0–8.0 24.0–26.0 3.0–5.0 ... ... N 0.24–0.32 Cu 0.50
F 54 S39274 25 chromium, 7 nickel, modified with nitrogen and tungsten 0.030 1.00 0.030 0.020 0.80 6.0–8.0 24.0–26.0 2.5–3.5 ... ... N 0.24–0.32 Cu 0.20–0.80 W 1.50–2.50
F 55 S32760 25 chromium, 7 nickel, 3.5 molybdenum, modified with nitrogen and tungsten 0.030 1.00 0.030 0.010 1.00 6.0–8.0 24.0–26.0 3.0–4.0 ... ... N 0.20–0.30 Cu 0.50–1.00 W 0.50–1.00Q
F 57 S39277 26 chromium, 7 nickel, 3.7 molybdenum 0.025 0.80 0.025 0.002 0.80 6.5–8.0 24.0–26.0 3.0–4.0 ... ... Cu 1.20–2.00 W 0.80–1.20 N 0.23–0.33
F 59 S32520 25 chromium, 6.5 nickel, 4 molybdenum with nitrogen 0.030 1.50 0.035 0.020 0.80 5.5–8.0 24.0–26.0 3.0–5.0 ... ... N 0.20–0.35 Cu 0.50–3.00

A182/A182M-11a

TABLE 2 Continued
Identification Symbol UNS Designation Grade Composition, %
Carbon Manganese Phosphorus Sulfur Silicon Nickel Chromium Molybdenum Columbium Titanium Other Elements
F 60 S32205 22 chromium, 5.5 nickel, 3 molybdenum, modified with nitrogen 2205G 0.030 2.00 0.030 0.020 1.00 4.5–6.5 22.0–23.0 3.0–3.5 ... ... N 0.14–0.20
F 61 S32550 26 chromium, 6 nickel, 3.5 molybdenum with nitrogen and copper 255G 0.040 1.50 0.040 0.030 1.00 4.5–6.5 24.0–27.0 2.9–3.9 ... ... Cu 1.50–2.50N 0.10–0.25
F 65 S32906 29 chromium, 6.5 nickel, 2 molybdenum with nitrogen 0.030 0.80–1.50 0.030 0.030 0.80 5.8–7.5 28.0–30.0 1.5–2.6 ... ... Cu 0.80N 0.30–0.40
F 66 S32202 22 chromium, 2.0 nickel, 0.25 molybdenum with nitrogen 0.030 2.00 0.040 0.010 1.00 1.00–2.80 21.5–24.0 0.45 ... ... N 0.18–0.26
F 67 S32506 25 chromium, 6 nickel, 3 molybdenum, with nitrogen and tungsten 0.030 1.00 0.040 0.015 0.90 5.5–7.2 24.0–26.0 3.0–3.5 ... ... N 0.08–0.20W 0.05–0.30
A Al l val u es are maxi m u m u n l ess othe rwise stated . Whe re e l l i pses ( . . . ) appear i n th is tabl e , the re is no req u i rement and analysis fo r the e l ement need not be dete rm i ned o r repo rted .
B G rade F 2 was fo rme rly assig ned to the 1 % ch rom i u m , 0 . 5 % molybden u m g rade wh ich is now G rade F 1 2 .
C The p resent g rade F 5a (0 . 25 max carbon) p revious to 1 955 was assig ned the identification sym bol F 5 . I dentification sym bol F 5 i n 1 955 was assig ned to the 0 . 1 5 max carbon g rade to be consistent with ASTM specifications fo r othe r p rod ucts such as p i pe , tu b i ng , bolti ng , we ld i ng fitti ngs , and the l i ke .

D
Appl ies to both heat and p rod uct analyses .

G Nam i ng system developed and appl ied by ASTM .

H G rade F XM -27Cb shal l have a n ickel pl us coppe r content of 0 . 50 max % . P rod uct analysis tole rance ove r the maxi m u m specified l i m it fo r carbon and n itrogen shal l be 0 . 002 % .

I G rades F 304 , F 304 L, F 3 1 6 , and F 3 1 6 L shal l have a maxi m u m n itrogen content of 0 . 1 0 % .

J G rades F 304 N , F 3 1 6 N , F 304 LN , and F 3 1 6 LN shal l have a n itrogen content of 0 . 1 0 to 0 . 1 6 % .

K G rade F 3 1 6Ti shal l have a titan i u m content not l ess than five ti mes the carbon pl us n itrogen content and not mo re than 0 . 70 % .

L G rade F 32 1 shal l have a titan i u m content of not l ess than five ti mes the carbon content and not mo re than 0 . 70 % .

M G rade F 32 1 H shal l have a titan i u m content of not l ess than fou r ti mes the carbon content and not mo re than 0 . 70 % .

N G rades F 347 and F 348 shal l have a col u m bi u m content of not l ess than ten ti mes the carbon content and not mo re than 1 . 1 0 % .

O G rades F 347 H and F 348 H shal l have a col u m bi u m content of not l ess than e i g ht ti mes the carbon content and not mo re than 1 . 1 0 % .

P
G rade F347 LN shal l have a col u m bi u m content of not l ess than 1 5 ti mes the carbon content .

Q % C r + 3 . 3 3 % M o + 1 6 3 % N = 40 m i n .

A182/A182M-11a

TABLE 3 Tensile and Hardness Requirements A
Grade Symbol Tensile Strength, min, ksi [MPa] Yield Strength, min, ksi [MPa]B Elongation in 2 in. [50 mm] or 4D, min, % Reduction of Area, min, % Brinell Hardness Number, HBW
Low Alloy Steels
F 1 70 [485] 40 [275] 20 30 143-192
F 2 70 [485] 40 [275] 20 30 143-192
F 5 70 [485] 40 [275] 20 35 143-217
F 5a 90 [620] 65 [450] 22 50 187-248
F 9 85 [585] 55 [380] 20 40 179-217
F 10 80 [550] 30 [205] 30 50 ...
F 91 90 [620] 60 [415] 20 40 190-248
F 92 90 [620] 64 [440] 20 45 269 max
F 122 90 [620] 58 [400] 20 40 250 max
F 911 90 [620] 64 [440] 18 40 187-248
F 11 Class 1 60 [415] 30 [205] 20 45 121-174
F 11 Class 2 70 [485] 40 [275] 20 30 143-207
F 11 Class 3 75 [515] 45 [310] 20 30 156-207
F 12 Class 1 60 [415] 32 [220] 20 45 121-174
F 12 Class 2 70 [485] 40 [275] 20 30 143-207
F 21 75 [515] 45 [310] 20 30 156-207
F 3V, and F 3VCb 85-110 [585-760] 60 [415] 18 45 174-237
F 22 Class 1 60 [415] 30 [205] 20 35 170 max
F 22 Class 3 75 [515] 45 [310] 20 30 156-207
F 22V 85-110 [585-780] 60 [415] 18 45 174-237
F 23 74 [510] 58 [400] 20 40 220 max
F 24 85 [585] 60 [415] 20 40 248 max
FR 63 [435] 46 [315] 25 38 197 max
F 36, Class 1 90 [620] 64 [440] 15 ... 252 max
F 36, Class 2 95.5 [660] 66.5 [460] 15 ... 252 max
Martensitic Stainless Steels
F 6a Class 1 70 [485] 40 [275] 18 35 143-207
F 6a Class 2 85 [585] 55 [380] 18 35 167-229
F 6a Class 3 110 [760] 85 [585] 15 35 235-302
F 6a Class 4 130 [895] 110 [760] 12 35 263-321
F 6b 110-135 [760-930] 90 [620] 16 45 235-285
F 6NM 115 [790] 90 [620] 15 45 295 max
Ferritic Stainless Steels
F XM-27Cb 60 [415] 35 [240] 20 45 190 max
F 429 60 [415] 35 [240] 20 45 190 max
F 430 60 [415] 35 [240] 20 45 190 max
Austenitic Stainless Steels
F 304 75 [515]C 30 [205] 30 50 ...
F 304H 75 [515]C 30 [205] 30 50 ...
F 304L 70 [485]D 25 [170] 30 50 ...
F 304N 80 [550] 35 [240] 30E 50F ...
F 304LN 75 [515]C 30 [205] 30 50 ...
F 309H 75 [515]C 30 [205] 30 50 ...
F 310 75 [515]C 30 [205] 30 50 ...
F 310MoLN 78 [540] 37 [255] 25 40 ...
F 310H 75 [515]C 30 [205] 30 50 ...
F 316 75 [515]C 30 [205] 30 50 ...
F 316H 75 [515]C 30 [205] 30 50 ...
F 316L 70 [485]D 25 [170] 30 50 ...
F 316N 80 [550] 35 [240] 30E 50F ...
F 316LN 75 [515]C 30 [205] 30 50 ...
F 316Ti 75 [515] 30 [205] 30 40 ...
F 317 75 [515]C 30 [205] 30 50 ...
F 317L 70 [485]D 25 [170] 30 50 ...
S31727 80 [550] 36 [245] 35 50 217
S32053 93 [640] 43 [295] 40 50 217
F 347 75 [515]C 30 [205] 30 50 ...
F 347H 75 [515]C 30 [205] 30 50 ...
F 347LN 75 [515] 30 [205] 30 50 ...
F 348 75 [515]C 30 [205] 30 50 ...
F 348H 75 [515]C 30 [205] 30 50 ...
F 321 75 [515]C 30 [205] 30 50 ...
F 321H 75 [515]C 30 [205] 30 50 ...
F XM-11 90 [620] 50 [345] 45 60 ...
TABLE 3 Continued
Grade Symbol Tensile Strength, min, ksi [MPa] Yield Strength, min, ksi [MPa]B Elongation in 2 in. [50 mm] or 4D, min, % Reduction of Area, min, % Brinell Hardness Number, HBW
F XM-19 100 [690] 55 [380] 35 55 ...
F 20 80 [550] 35 [240] 30 50 ...
F 44 94 [650] 44 [300] 35 50 ...
F 45 87 [600] 45 [310] 40 50 ...
F 46 78 [540] 35 [240] 40 50 ...
F 47 75 [525] 30 [205] 40 50 ...
F 48 80 [550] 35 [240] 40 50 ...
F 49 115 [795] 60 [415] 35 40 ...
F 56 73 [500] 27 [185] 30 35 ...
F 58 109 [750] 61 [420] 35 50 ...
F 62 95 [655] 45 [310] 30 50 ...
F 63 80 [550] 32 [220] 25 ... 192 max
F 64 90 [620] 40 [275] 35 50 217 max
F 904L 71 [490] 31 [215] 35 ... ...
Ferritic-Austenitic Stainless Steels
F 50 100–130 [690–900] 65 [450] 25 50 ...
F 51 90 [620] 65 [450] 25 45 ...
F 52 100 [690] 70 [485] 15 ... ...
F 53 116 [800]G 80 [550]G 15 ... 310 max
F 54 116 [800] 80 [550] 15 30 310 max
F 55 109–130 [750–895] 80 [550] 25 45 ...
F 57 118 [820] 85 [585] 25 50 ...
F 59 112 [770] 80 [550] 25 40 ...
F 60 95 [655] 65 [450] 25 45 ...
F 61 109 [750] 80 [550] 25 50 ...
F 65 109 [750] 80 [550] 25 ... ...
F 66 94 [650] 65 [450] 30 ... 290 max
F 67 90 [620] 65 [450] 18 ... 302
A Where ellipses appear in this table, there is no requirement and the test for the value need neither be performed nor a value reported.
B Determined by the 0.2 % offset method. For ferritic steels only, the 0.5 % extension-under-load method may also be used.
C For sections over 5 in. [130 mm] in thickness, the minimum tensile strength shall be 70 ksi [485 MPa].
D For sections over 5 in. [130 mm] in thickness, the minimum tensile strength shall be 65 ksi [450 MPa].
E Longitudinal. The transverse elongation shall be 25 % in 2 in. or 50 mm, min.
F Longitudinal. The transverse reduction of area shall be 45 % min.
G For sections over 2 in. [50 mm] in thickness, the minimum tensile strength shall be 106 ksi [730 MPa]; the minimum yield strength shall be 75 ksi [515 MPa].

9.7.2 The Charpy V-notch test specimens shall be obtained as required for tension tests in 9.2, 9.3 and 9.5. One set of three Charpy V-notch specimens shall be taken from each tensile specimen location.

9.7.3 The longitudinal axis and mid-length of impact specimen shall be located similarly to the longitudinal axis of the tension test specimens. The axis of the notch shall be normal to the nearest heat-treated surface of the forging.

9.7.4 The Charpy V-notch tests shall meet a minimum energy absorption value of 40 ft-lbf [54 J] average of three specimens. One specimen only in one set may be below 40 ft-lbf [54 J], and it shall meet a minimum value of 35 ft-lbf [48 J].

9.7.5 The impact test temperature shall be 0°F [-18°C]

10 Grain Size for Austenitic Grades

10.1 All H grades and grade F 63 shall be tested for average grain size by Test Methods E112.

10.1.1 Grades F 304H, F 309H, F 310H, and F 316H shall have a grain size of ASTM No. 6 or coarser.

10.1.2 Grades F 321H, F 347H, and F 348H shall have a grain size of ASTM No. 7 or coarser.

10.1.3 Grade F 63 shall have a grain size of ASTM No. 3 or finer.

11 Corrosion Testing for Austenitic Grades

11.1 Corrosion testing is not required by this specification.

11.2 Austenitic grades shall be capable of meeting the intergranular corrosion test requirements described in Supplementary Requirement S4.

12 Retreatment

12.1 If the results of the mechanical tests do not conform to the requirements specified, the manufacturer may reheat treat the forgings and repeat the tests specified in Section 9.

13 Nondestructive Test Requirements

13.1 Hollow forgings of Grades F 91, F 92, F 122, and F 911, NPS 4 [DIN 100] and larger, whose internal surfaces are not accessible to magnetic particle or liquid penetrant examination, shall be examined by an ultrasonic test in accordance with Practice A388/A388M.

13.2 Hollow forgings of Grades F 91, F 92, F 122, and F 911, NPS 4 [DIN 100] and larger, whose internal surfaces are accessible to magnetic particle or liquid penetrant examination, shall be examined on their internal surfaces by either a magnetic particle test in accordance with Practice A275/ A275M, or by a liquid penetrant examination in accordance with Test Method E165, as applicable.

13.3 Time of Examination:

13.3.1 Examination by one of the methods in 13.1 or 13.2, for specification acceptance, shall be performed after all mechanical processing and heat treatment. This requirement does not preclude additional testing at earlier stages in the processing.

13.4 Evaluation of Imperfections Found by Ultrasonic Examination:

13.4.1 Forgings producing a signal equal to or greater than the lowest signal produced by the reference discontinuities shall be identified and separated from the acceptable forgings. The area producing the signal may be reexamined.

13.4.3 If the test signals were produced by visual imperfections such as scratches, surface roughness, dings, tooling marks, cutting chips, steel die stamps, or stop marks, the forging is permitted to be accepted based upon visual examination provided that the depth of the imperfection is less than 0.004 in. [0.1 mm] or 12.5 % of the specified wall thickness, whichever is the greater.

13.5 Treatment of Imperfections Found by Magnetic Particle or Liquid Penetrant Examination:

13.5.1 Defects shall be completely removed prior to weld repair by chipping or grinding to sound metal. Removal of these defects shall be verified by magnetic particle inspection in accordance with Test Method A275/A275M or by liquid penetrant inspection in accordance with Test Method E165.

13.5.2 Rejected forgings may be reconditioned and retested, provided that the wall thickness is not decreased to less than that required by this specification and the purchase order. The outside diameter at the point of grinding may be reduced by the amount so removed. To be accepted, retested forgings shall meet the test requirement.

13.5.3 If the imperfection is explored to the extent that it can be identified as non-rejectable, the forging may be accepted without further test provided that the imperfection does not encroach on the minimum required wall thickness.

14 Workmanship, Finish, and Appearance

14.1 Forgings shall conform to the requirements of Specification A961/A961M.

14.2 The forgings shall be free of scale, machining burrs which might hinder fit-up, and other injurious imperfections as defined herein. The forgings shall have a workmanlike finish,

and machined surfaces (other than surfaces having special requirements) shall have a surface finish not to exceed 250 AA (arithmetic average) roughness height.

15 Repair by Welding

15.1 Weld repairs shall be permitted (see Supplementary Requirement S58 of Specification A961/A961M) at the discretion of the manufacturer with the following limitations and requirements:

15.1.1 The welding procedure and welders shall be qualified in accordance with Section IX of the ASME Boiler and Pressure Vessel Code.

15.1.2 The weld metal shall be deposited using the electrodes specified in Table 4 except as otherwise provided in Supplementary Requirement S5. The electrodes shall be purchased in accordance with AWS Specifications A5.4/A5.4M, A5.5/A5.5M, A5.9/A5.9M, A5.11/A5.11M, A5.14/A5.14M, A5.23/A5.23M, A5.28/A5.28M, or A5.29/A5.29M. The submerged arc process with neutral flux, the gas metal-arc process, the gas tungsten-arc process, and gas shielded processes using flux-core consumables, may be used.

15.1.3 Defects shall be completely removed prior to welding by chipping or grinding to sound metal as verified by magnetic-particle inspection in accordance with Test Method A275/A275M for the low alloy steels and ferritic, martensitic, or ferritic-austenitic stainless steels, or by liquid-penetrant inspection in accordance with Test Method E165 for all grades.

15.1.4 After repair welding, the welded area shall be ground smooth to the original contour and shall be completely free of defects as verified by magnetic-particle or liquid-penetrant inspection, as applicable.

15.1.5 The preheat, interpass temperature, and post-weld heat treatment requirements given in Table 4 shall be met. Austenitic stainless steel forgings may be repair-welded without the post-weld heat treatment of Table 4, provided purchaser approval is obtained prior to repair.

15.1.6 Repair by welding shall not exceed 10 % of the surface area of the forging nor 33
1
⁄3 % of the wall thickness of the finished forging or 3
⁄8 in. [9.5 mm], whichever is less, without prior approval of the purchaser.

15.1.7 When approval of the purchaser is obtained, the limitations set forth in 15.1.6 may be exceeded, but all other requirements of Section 15 shall apply.

15.1.8 No weld repairs are permitted for F 6a Classes 3 and 4.

15.1.9 Post-weld heat treatment times for F 36 are: for Class 1, up to 2 in. [50 mm] in thickness, 1 h per in. [25 mm], 15 minutes minimum, and over 2 in. [50 mm], 15 minutes for each additional in. of thickness or fraction thereof; for Class 2, 1 h per in. [25 mm], 1⁄2 h minimum.

TABLE 4 Repair Welding Requirements
Grade Symbol ElectrodesA Recommended Preheat and Interpass Temperature Range, °F [°C] Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C]
Low Alloy Steels
F 1 E 7018-A 1 200–400 [95–205] 1150 [620]
F 2 E 8018-B 1 300–600 [150–315] 1150 [620]
TABLE 4 Continued
Grade Symbol ElectrodesA Recommended Preheat and Interpass Temperature Range, °F [°C] Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C]
F 5 E80XX-B6, where XX can be 15, 16, or 18 400-700 [205-370] 1250 [675]
F 5a E80XX-B6, where XX can be 15, 16, or 18 400-700 [205-370] 1250 [675]
F 9 E80XX-B8, where XX can be 15, 16, or 18 400-700 [205-370] 1250 [675]
F 10B ... ... ...
F 91 ...C 400-700 [205-370] 1350-1470 [730-800]
F 92 ...D 400-700 [205-370] 1350-1470 [730-800]
F 122 ...D 400-700 [205-370] 1350-1470 [730-800]
F 911 ...D 400-700 [205-370] 1365-1435 [740-780]
F 11, Class 1, 2, and 3 E 8018-B 2 300-600 [150-315] 1150 [620]
F 12, Class 1 and 2 E 8018-B 2 300-600 [150-315] 1150 [620]
F 21 E 9018-B 3 300-600 [150-315] 1250 [675]
F 3V, and F 3VCb 3 % Cr, 1 % Mo, 1⁄4 % V-Ti 300-600 [150-315] 1250 [675]
F 22 Class 1 E 9018-B 3 300-600 [150-315] 1250 [675]
F 22 Class 3 E 9018-B 3 300-600 [150-315] 1250 [675]
F 22V 2.25 % Cr, 1 % Mo, 0.25 % V-Cb 300-600 [150-315] 1250 [675]
F 23 2.25 % Cr, 1.6 % W, 0.25 % V-Mo-Cb-B 300-600 [150-315] 1350-1470 [730-800]
F 24 2.25 % Cr, 1 % Mo, 0.25 % V 200-400 [95-205]E 1350-1470 [730-800]E
F 36, Class 1 1.15 Ni, 0.65 Cu, Mo, Cb 400-700 [205-370] 1100-1200 [595-650]
F 36, Class 2 1.15 Ni, 0.65 Cu, Mo, Cb 400-700 [205-370] 1000-1150 [540-620]
Martensitic Stainless Steels
F 6a, Class 1 E 410-15 or 16 400-700 [205-370] 1250 [675]
F 6a, Class 2 E 410-15 or 16 400-700 [205-370] 1250 [675]
F 6b 13 % Cr, 11⁄2 % Ni, 1⁄2 % Mo 400-700 [205-370] 1150 [620]
F 6NM 13 % Cr, 4 % Ni 300-700 [150-370] 1050 [565]
Ferritic Stainless Steels
F XM-27Cb 26 % Cr, 1 % Mo NRF NR
F 429 E 430-16 400-700 [205-370] 1400 [760]
F 430 E 430-16 NR 1400 [760]
FR E 8018-C2 NR NR
Austenitic Stainless Steels
F 304 E 308-15 or 16 NR 1900 [1040] + WQG
F 304L E 308L-15 or 16 NR 1900 [1040] + WQ
F 304H E 308-15 or 16H or E308H-XX NR 1900 [1040] + WQ
F 304N E 308-15 or 16 NR 1900 [1040] + WQ
F 304LN E 308L-15 or 16 NR 1900 [1040] + WQ
F 309H E 309-15 or 16H or E309H-XX NR 1900 [1040] + WQ
F 310 E 310-15 or 16 NR 1900 [1040] + WQ
F 310H E 310-15 or 16H NR 1900 [1040] + WQ
F 310MoLN E 310Mo-15 or 16 NR 1920-2010 [1050-1100] + WQ
F 316 E 316-15 or 16 NR 1900 [1040] + WQ
F 316L E 316L-15 or 16 NR 1900 [1040] + WQ
F 316H E 316-15 or 16H or E316H-XX NR 1900 [1040] + WQ
F 316N E 316-15 or 16 NR 1900 [1040] + WQ
F 316LN E 316L-15 or 16 NR 1900 [1040] + WQ
F 316Ti E 316-15 or 16 NR 1900 [1040] + WQ
F 317 E 317-15 or 16 NR 1900 [1040] + WQ
F 317L E 317L-15 or 16 NR 1900 [1040] + WQ
S31727 ... NR ...
S32053 ... NR ...
F 321B E 347-15 or 16 NR 1900 [1040] + WQ
F 321HB E 347-15 or 16H NR 1925 [1050] + WQ
F 347 E 347-15 or 16 NR 1900 [1040] + WQ
F 347H E 347-15 or 16H NR 1925 [1050] + WQ
F 347LNf E 347-15 or 16 NR ...
E 348 E 347-15 or 16 NR 1900 [1040] + WQ
F 348H E 347-15 or 16H NR 1925 [1050] + WQ
F XM-11 XM-10W NR NR
F XM-19 XM-19W NR NR
F 20 E/ER-320, 320LR NR 1700-1850 [925-1010] + WQ
F 44 E NiCrMo-3 NR 2100 [1150] + WQ
F 45B ... ... ...
F 46 ... ... ...
F 47 ...J ... 2100 [1150] + WQ
TABLE 4 Continued
Grade Symbol ElectrodesA Recommended Preheat and Interpass Temperature Range, °F [°C] Post Weld Heat-Treatment Temperature, Minimum or Range, °F [°C]
F 48 ...J ... 2100 [1150] + WQ
F 49 ...J ... 2100 [1150] + WQ
F 58 E NiCrMo-10 ... 2100 [1150] + WQ
F 62 E NiCrMo-3 NR 2025 [1105] + WQ
F 904L E NiCrMo-3 NR 1920–2100 [1050–1150] + WQ
Ferritic-Austenitic Stainless Steels
F 50 25 % Cr, 6 % Ni, 1.7 % Mo NR NR
F 51 22 % Cr, 5.5 % Ni, 3 % Mo NR NR
F 52 26 % Cr, 8 % Ni, 2 % Mo NR NR
F 53 25 % Cr, 7 % Ni, 4 % Mo NR NR
F 54 25 % Cr, 7 % Ni, 3 % Mo, W NR NR
F 55 25 % Cr, 7 % Ni, 3.5 % Mo NR NR
F 57 25 % Cr, 7 % Ni, 3 % Mo, 1.5 % Cu, 1 % W NR NR
F 59 E Ni CrMo-10 NR NR
F 60 22 % Cr, 5.5 % Ni, 3 % Mo NR NR
F 61 26 % Cr, 9 % Ni, 3.5 % Mo NR NR
F 65 29 % Cr, 6.5 % Ni, 2 % Mo NR NR
F 66 22 % Cr, 2 % Ni, 0.25 % Mo NR NR
F 67 ... NR NR
A Except for Grades F 91, F 92, F 911, F 122, F 47, F 48, and F 49, electrodes shall comply with AWS Specifications A5.4/A5.4M, A5.5/A5.5M, A5.9/A5.9M, A5.11/A5.11M, A5.14/A5.14M, A5.23/A5.23M, or A5.28/A5.28M.
B Purchaser approval required.
C All repairs in F 91 shall be made with one of the following welding processes and consumables: SMAW, A5.5/A5.5M E90XX-B9; SAW, A5.23/A5.23M EB9 + flux; GTAW, A5.28/A5.28M ER90S-B9; and FCAW, A5.29/A5.29M E91T1-B9. In addition, the sum of the Ni+Mn content of all welding consumables shall not exceed 1.0 %.
D All repairs in F 92, F 911, and F 122, shall be made using welding consumables meeting the chemical requirements for the grade in Table 2.
E Preheat and PWHT are not required for this grade for forgings whose section thickness does not exceed 0.500 in. [12.7 mm].
F NR = not required.
G WQ = water quench.
H Filler metal shall additionally have 0.04 % minimum carbon.
I Matching filler metal is available.
J Match filler metal is available. Fabricators have also used AWS A5.14/A5.14M, Classification ERNiCrMo-3 and AWS A5.11/A5.11M, Class E, ENiCrMo-3 filler metals.

16 Inspection

16.1 Inspection provisions of Specification A961/A961M apply.

17 Rejection and Rehearing

17.1 The purchaser shall comply with the provisions of Specification A961/A961M.

18 Certification

18.1 In addition to the certification requirements of Specification A961/A961M, test reports shall be furnished to the purchaser or his representative.

18.2 Test reports shall include certification that all requirements of this specification have been met. The specification designation included on test reports shall include year of issue and revision letter, if any. The manufacturer shall provide the following where applicable:

18.2.1 Type heat treatment, Section 7,

18.2.2 Product analysis results, Section 8 of Specification A961/A961M,

18.2.3 Tensile property results, Section 9 (Table 3), report the yield strength and ultimate strength, in ksi [MPa], elongation and reduction in area, in percent,

18.2.4 Chemical analysis results, Section 8 (Table 2),

18.2.5 Hardness results, Section 9 (Table 3, and for F23, Tables 2 and 3),

18.2.6 Grain size results, Section 10, and

18.2.7 Any supplementary testing required by the purchase order.

19 Product Marking

19.1 In addition to the marking requirements of Specification A961/A961M, the manufacturer’s name (see Note 3) or symbol shall be permanently marked on each forging. NOTE 3—For purposes of identification marking, the manufacturer is considered the organization that certifies the piping component was manufactured, sampled, and tested in accordance with this specification, and the results have been determined to meet the requirements of this specification.

19.1.1 Quenched and tempered low alloy or martensitic stainless forgings shall be stamped with the letters QT following the specification designation.

19.1.2 Forgings repaired by welding shall be marked with the letter “W” following the Specification designation. When repair-welded austenitic stainless steel forgings have not been postweld heat treated in accordance with Table 4, the letters “WNS” shall be marked following the specification designation.

19.1.3 When test reports are required, the markings shall consist of the manufacturer’s symbol or name, the grade symbol, and such other markings as necessary to identify the part with the test report (19.1.1 and 19.1.2 shall apply).

19.1.4 Parts meeting all requirements for more than one class or grade may be marked with more than one class or grade designation such as F 304/F 304H, F 304/F 304L, and the like.

19.2 Bar Coding—In addition to the requirements in 19.1, bar coding is acceptable as a supplemental identification method. The purchaser may specify in the order a specific bar coding system to be used. The bar coding system, if applied at the discretion of the supplier, should be consistent with one of the published industry standards for bar coding. If used on small parts, the bar code may be applied to the box or a substantially applied tag.

20 Keywords

20.1 austenitic stainless steel; chromium alloy steel; chromium-molybdenum steel; ferritic/austenitic stainless steel; ferritic stainless steel; martensitic stainless steel; nickel alloy steel; notch toughness requirements; pipe fittings; piping applications; pressure containing parts; stainless steel fittings; stainless steel forgings; steel; steel flanges; steel forgings, alloy; steel valves; temperature service applications, elevated; temperature service applications, high; wrought material

SUPPLEMENTARY REQUIREMENTS

In addition to any of the supplementary requirements of Specification A961/A961M, the following supplementary requirements shall apply only when specified by the purchaser in the order.

S1. Macroetch Test

S1.1 A sample forging shall be sectioned and etched to show flow lines and internal imperfections. The test shall be conducted according to Test Method E340. Details of the test shall be agreed upon between the manufacturer and the purchaser.

S2. Heat Treatment Details

S2.1 The manufacturer shall furnish a detailed test report containing the information required in 18.2 and shall include all pertinent details of the heat-treating cycle given the forgings.

S3. Material for Optimum Resistance to Stress-Corrosion Cracking

S3.1 Austenitic stainless steel shall be furnished in the solution-annealed condition as a final operation with no subsequent cold working permitted, except, unless specifically prohibited by the purchaser, straightening of bars from which parts are machined is permitted to meet the requirements of Specification A484/A484M.

S4. Corrosion Tests

S4.1 All austenitic stainless steels shall pass intergranular corrosion tests performed in accordance with Practice E of Practices A262.

S4.2 Intergranular corrosion tests shall be performed on specimens of ferritic stainless steels as described in Practices A763.

S4.3 For both the austenitic and ferritic stainless steels, details concerning the number of specimens and their source and location are to be a matter of agreement between the manufacturer and the purchaser.

S5. Special Filler Metal

S5.1 In repair-welded F 316, F 316L, F 316H, and F 316N forgings, the deposited weld metal shall conform to E 308

composition wire. Forgings repair welded with E 308 weld metal shall be marked F __ W 308.

S6. Hardness Test

S6.1 Each forging shall be hardness tested and shall meet the requirements of Table 3.

S8. Heat Treatment of Austenitic Forgings

S8.1 The purchaser shall specify the heat-treatment method (in 7.1 or in 7.3.1) that shall be employed.

S8.2 The manufacturer shall provide a test report containing the information required in 18.2 and shall include a statement of the heat-treatment method employed.

S9. Grain Size for Austenitic Grades

S9.1 Forgings made from austenitic grades other than H grades shall be tested for average grain size by Test Method E112. Details of the test shall be agreed upon between the manufacturer and the purchaser.

S10. Stabilization Treatment

S10.1 Subsequent to the solution anneal for Grades F 321, F 321H, F 347, F 347H, F 348, and F 348H, these grades shall be given a stabilization heat treatment at 1500 to 1600 °F [815 to 870 °C] for a minimum of 2 h/in. [4.7 min/mm] of thickness and then cooling in the furnace or in air. In addition to the marking required in Section 19, the grade designation symbol shall be followed by the symbol “S10.”

S11. Grain Size Requirements for Non-H-Grade Austenitic Steels Used Above 1000 °F [540 °C]

S11.1 Non-H grades of austenitic stainless steels shall have a grain size of No. 7 or coarser as determined in accordance with Test Methods E112. The grain size so determined shall be on a certified test report.

资源下载此资源下载价格为5金币立即购买,VIP免费

1.本站大部份文档均属免费,部份收费文档,经过本站分类整理,花了精力和时间,收费文档是为了网站运营成本等费用开支;
2.购买会员:全部免费下载本站资源(或单次下载)即视为对网站的赞助、打赏,非商业交易行为(不认同此观点请勿支付)请慎重考虑;
3.所有收费文档都真实可靠,为了节约成本,文档在网站前台不做预览,如果付费后,与实际文档不符合,都可以加微信号:pdftj888申请退款;
4.付费下载过程中,如果遇到下载问题,都可以加微信号pdftj888解决;
5.手机支付,尽量选择支付宝支付;
6.如图集或者标准不清楚,在本站找不到您需要的规范和图集,希望增加资料等任何问题,可联系微信号:pdftj888解决;

文档天下
  • 本文由 发表于 2026年11月24日 08:41:23
  • 转载请务必保留本文链接:https://www.998pdf.com/84170.html
匿名

发表评论

匿名网友 填写信息

:?: :razz: :sad: :evil: :!: :smile: :oops: :grin: :eek: :shock: :???: :cool: :lol: :mad: :twisted: :roll: :wink: :idea: :arrow: :neutral: :cry: :mrgreen: