ASTM A194 A194M-16a Standard Specification for Carbon Steel, Alloy Steel, and Stainless Steel Nuts f

文档天下 国外标准评论1阅读模式

1 Scope*

1.1 This specification
2 covers a variety of carbon, alloy, and martensitic stainless steel nuts in the size range 1⁄4 through 4 in. and metric M6 through M100 nominal. It also covers austenitic stainless steel nuts in the size range 1⁄4 in. and M6 nominal and above. These nuts are intended for high-pressure or hightemperature service, or both. Grade substitutions without the purchaser’s permission are not allowed.

1.2 Bars from which the nuts are made shall be hot-wrought. The material may be further processed by centerless grinding or by cold drawing. Austenitic stainless steel may be solution annealed or annealed and strain-hardened. When annealed and strain hardened austenitic stainless steel is ordered in accordance with Supplementary Requirement S1, the purchaser should take special care to ensure that 8.2.2, Supplementary Requirement S1, and Appendix X1 are thoroughly understood.

1.3 Supplementary requirements of an optional nature are provided. These shall apply only when specified in the inquiry, contract, and order.

1.4 This specification is expressed in both inch-pound units and in SI units. However, unless the order specifies the applicable “M” specification designation (SI units), the material shall be furnished to inch-pound units.

1.5 The values stated in either inch-pound units or SI units are to be regarded separately as standard. The values stated in each system may not be exact equivalents; therefore, each system shall be used independently of the other. Combining values from the two systems may result in non-conformance with the standard. Within the text, the SI units are shown in brackets.

2 Referenced Documents

2.1 ASTM Standards:
3

A153/A153M Specification for Zinc Coating (Hot-Dip) on Iron and Steel Hardware

A276/A276M Specification for Stainless Steel Bars and Shapes

A320/A320M Specification for Alloy-Steel and Stainless Steel Bolting for Low-Temperature Service

A370 Test Methods and Definitions for Mechanical Testing of Steel Products

A962/A962M Specification for Common Requirements for Bolting Intended for Use at Any Temperature from Cryogenic to the Creep Range

B633 Specification for Electrodeposited Coatings of Zinc on Iron and Steel

B695 Specification for Coatings of Zinc Mechanically Deposited on Iron and Steel

B696 Specification for Coatings of Cadmium Mechanically Deposited

B766 Specification for Electrodeposited Coatings of Cadmium

E112 Test Methods for Determining Average Grain Size

E566 Practice for Electromagnetic (Eddy Current) Sorting of Ferrous Metals

F606/F606M Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners, Washers, Direct Tension Indicators, and Rivets

F1940 Test Method for Process Control Verification to Prevent Hydrogen Embrittlement in Plated or Coated Fasteners

F1941/F1941M Specification for Electrodeposited Coatings on Mechanical Fasteners, Inch and Metric

F2329/F2329M Specification for Zinc Coating, Hot-Dip, Requirements for Application to Carbon and Alloy Steel

1 This specification is under the jurisdiction of ASTM Committee A01 on Steel, Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee A01.22 on Steel Forgings and Wrought Fittings for Piping Applications and Bolting Materials for Piping and Special Purpose Applications.

Current edition approved Dec. 1, 2016. Published December 2016. Originally approved in 1936. Last previous edition approved in 2016 as A194/A194M – 16. DOI: 10.1520/A0194_A0194M-16A.

2 For ASME Boiler and Pressure Vessel Code applications see related Specification SA-194 in Section II of that code.

3 For referenced ASTM standards, visit the ASTM website, www.astm.org, or contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM Standards volume information, refer to the standard’s Document Summary page on the ASTM website.

Bolts, Screws, Washers, Nuts, and Special Threaded Fasteners

2.2 ASME Standards:
4

B 1.1 Unified Screw Threads

B 1.2 Gages and Gaging for Unified Inch Screw Threads

B 1.13M Metric Screw Threads

B 18.2.2 Square and Hex Nuts

B 18.2.4.6M Metric Heavy Hex Nuts

2.3 ISO Standards:
5

4033 Hexagon High Nuts (Style 2) – Product A and B

3 Terminology

3.1 Definitions of Terms Specific to This Standard:

3.1.1 Austenitic Grades—All grades with a prefix of “8” or “9.”

3.1.2 Ferritic Grades—Grades 1, 2, 2H, 2HM, 3, 4, 6, 6F, 7, 7M, and 16.

3.1.3 Lot—Unless otherwise specified (see Discussion below), a lot is the quantity of nuts of a single nominal size and grade produced by the same manufacturing process.

3.1.3.1 Discussion—When Supplementary Requirement S5 is invoked on the purchase order, the following definitions of a lot shall apply:

3.1.3.2 For Grade 8 Nuts—The quantity of all the nuts of a single nominal diameter and grade made from the same heat of steel and made by the same manufacturing process.

3.1.3.3 For All Other Grade Nuts—(see 8.2 and 8.1.2.1)—All the nuts of a single nominal diameter and grade made from the same heat number and heat treated in the same batch if batch-type heat treating equipment is used or heat treated in the same continuous run of not more than 8 h under the same conditions if continuous-type heat treating equipment is used.

3.1.4 Type:

3.1.4.1 For Grade 8 Nuts—Variations within the grade designated by a letter and differentiated by chemistry and by manufacturing process.

3.1.4.2 For Grade 6 Nuts—Variations within the grade designated by the letter F as differentiated by chemical additions made for machineability.

3.1.5 Series—The dimensional relationship and geometry of the nuts as described in ASME B 18.2.2 for inch nuts and ISO 4033 for metric nuts sizes M6 through M10 and ASME B 18.2.4.6M for nuts sizes M12 through M100.

4 Ordering Information

4.1 The inquiry and order for bolting material and bolting components under this specification shall include the following as required to describe the items adequately:

4.1.1 Specification designation, year date, and grade, issue date and revision letter,

4.1.2 Quantity, number of pieces,

4 Available from American Society of Mechanical Engineers (ASME), ASME International Headquarters, Two Park Ave., New York, NY 10016-5990, http:// www.asme.org.

5 Available from International Organization for Standardization (ISO), 1, ch. de la Voie-Creuse, CP 56, CH-1211 Geneva 20, Switzerland, http://www.iso.org.

4.1.3 Dimensions (see Section 9),

4.1.4 Options in accordance with 8.2.2.1, 9.1, 9.2, 10.3, and 12, and

4.1.5 Supplementary Requirements, if any.

4.2 Coatings—Coatings are prohibited unless specified by the purchaser (see Supplementary Requirements S7 and S8). When coated nuts are ordered, the purchaser should take special care to ensure that Appendix X2 is thoroughly understood.

4.3 See Supplementary Requirement S3 for nuts to be used in low temperature applications (Specification A320/A320M).

4.4 Proof Load Testing—See Supplementary Requirement S9 for proof load testing of nuts manufactured to dimensions and configurations other than those covered in Tables 3 and 4.

5 Common Requirements

5.1 Bolting material and bolting components supplied to this specification shall conform to the requirements of Specification A962/A962M, of which nuts are considered bolting components, as are bolts, studs, screws, and washers intended for use in special service applications. These requirements include test methods, finish, thread dimensions, marking, certification, optional supplementary requirements, and others. Failure to comply with the requirements of Specification A962/A962M constitutes nonconformance with this specification. In case of conflict between the requirements of this specification and Specification A962/A962M, this specification shall prevail.

6 Manufacture (Process)

6.1 Stainless steels for all types of Grade 6 and 8 nuts shall be made by one of the following processes:

6.1.1 Electric-furnace (with separate degassing and refining optional),

6.1.2 Vacuum induction furnace, or

6.1.3 Either of the above followed by electroslag remelting, or consumable-arc remelting.

6.2 The steel producer shall exercise adequate control to eliminate excessive unhomogeneity, nonmetallics, pipe, porosity, and other defects.

6.3 Grades 1 and 2 nuts shall be hot or cold forged, or shall be machined from hot-forged, hot-rolled, or cold-drawn bars.

6.3.1 All Grade 1 and 2 nuts shall be stress-relieved at a temperature of at least 1000 °F [538 °C] after forming or machining from bar with the following exceptions:

6.3.1.1 Nuts made by hot forging.

6.3.1.3 Nuts machined from hot-forged/hot-rolled and coldfinished (max 10 % reduction in area) bar.

6.3.1.2 Nuts machined from hot-forged or hot-rolled bar.

6.3.1.4 Nuts machined from cold-drawn and annealed (min 1000 °F [538 °C]) bar.

6.3.2 Grade 1 and 2 nuts made by hot forging or by machining from hot-forged or hot-rolled bars need not be stress relieved.

6.4 Grades 2H, 2HM, 3, 4, 6, 6F, 7, 7M, and 16 nuts shall be hot- or cold-forged or shall be machined from hot-forged,

TAB LE 1 Chem ical Req u i rements A,B,C,D
Grade Symbol Material UNS Number Carbon, % Manganese, % Phosphorus, % Sulfur, E % Silicon, % Chromium, % Nickel, % Molybdenum, % Titanium, % Columbium, H, % Nitrogen, % Other Elements, %
1 carbon 0.15 min 1.00 0.040 0.050 0.40 ... ... ... ... ... ... ...
2, 2HM, and 2H carbon 0.40 min 1.00 0.040 0.050 0.40 ... ... ... ... ... ... ...
4G carbon, molybdenum 0.40–0.50 0.70–0.90 0.035 0.040 0.15–0.35 ... ... 0.20–0.30 ... ... ... ...
3 Type 501 0.10 min 1.00 0.040 0.030 1.00 4.0–6.0 ... 0.40–0.65 ... ... ... ...
6 Type 410 S41000 0.08–0.15 1.00 0.040 0.030 1.00 11.5–13.5 ... ... ... ... ... ...
6F Type 416 S41600 0.15 1.25 0.060 0.15 min 1.00 12.0–14.0 ... ... ... ... ... ...
6F Type 416Se S41623 0.15 1.25 0.060 0.060 1.00 12.0–14.0 ... ... ... ... Selenium, 0.15 min
7, 7M Type 4140/4142/4145,4140H,4142H,4145H 0.38–0.48 0.75–1.0 0.035 0.04 0.15–0.35 0.80–1.10 ... 0.15–0.25 ... ... ... ...
8, 8A Type 304 S30400 0.08 2.00 0.045 0.030 1.00 18.0–20.0 8.0–11.0 ... ... ... ... ...
8C, 8CA Type 347 S34700 0.08 2.00 0.045 0.030 1.00 17.0–19.0 9.0–12.0 ... ... 10 x carbon content, min 1.10 ... ...
8CLN, 8CLNA Type 347LN S34751 0.005–0.020 2.00 0.045 0.030 1.00 17.0–19.0 9.0–13.0 ... ... 0.20–0.50, 15 x carbon content, min 0.06–0.10 ...
8M, 8MA Type 316 S31600 0.08 2.00 0.045 0.030 1.00 16.0–18.0 10.0–14.0 2.00–3.00 ... ... ... ...
8T, 8TA Type 321 S32100 0.08 2.00 0.045 0.030 1.00 17.0–19.0 9.0–12.0 ... 5 x (C+N) min - 0.70 max ... 0.10 ...
8F, 8FA Type 303 S30300 0.15 2.00 0.20 0.15 min 1.00 17.0–19.0 8.0–10.0 ... ... ... ... ...
8F, 8FA Type 303Se S30323 0.15 2.00 0.20 0.06 1.00 17.0–19.0 8.0–10.0 ... ... ... Selenium, 0.15 min
8P, 8PA Type 305 S30500 0.12 2.00 0.045 0.030 1.00 17.0–19.0 11.0–13.0 ... ... ... ... ...
8N, 8NA Type 304N S30451 0.08 2.00 0.045 0.030 1.00 18.0–20.0 8.0–11.0 ... ... ... 0.10–0.16
8LN, 8LNA Type 304LN S30453 0.030 2.00 0.045 0.030 1.00 18.0–20.0 8.0–11.0 ... ... ... 0.10–0.16
8MN, 8MNA Type 316N S31651 0.08 2.00 0.045 0.030 1.00 16.0–18.0 10.0–13.0 2.00–3.00 ... ... 0.10–0.16
8MLN, 8MLNA Type 316LN S31653 0.030 2.00 0.045 0.030 1.00 16.0–18.0 10.0–13.0 2.00–3.00 ... ... 0.10–0.16
8R, 8RAF XM19 S20910 0.06 4.0–6.0 0.045 0.030 1.00 20.5–23.5 11.5–13.5 1.50–3.00 ... 0.10–0.30 0.20–0.40 Vanadium, 0.10–0.30
8S, 8SA S21800 0.10 7.0–9.0 0.060 0.030 3.5–4.5 16.0–18.0 8.0–9.0 ... ... ... 0.08–0.18
8MLCuN, 8MLCuNA S31254 S31254 0.020 1.00 0.030 0.010 0.80 19.5–20.5 17.5–18.5 6.0–6.5 ... ... 0.18–0.22 Copper, 0.50–1.00
B8ML4CuN S31730 S31730 0.030 2.00 0.040 0.010 1.00 17.0–19.0 15.0–16.5 3.0–4.0 ... ... 0.045 Copper 4.0–5.0
9C, 9CA N08367 N08367 0.030 2.00 0.040 0.030 1.00 20.0–22.0 23.5–25.5 6.0–7.0 0.18–0.25 Copper 0.75

A194/A194M - 16a

TABLE 1 Continued
SGyrmadbeol Mate rial N uUmNbSe r Car%bon , Mnaensgea, - Phorussp,ho- S u %lfu r, E S i l i%con ,% % Ch ro%m i u m , N ic%kel , dMeonluymb-, nTi uitam-, bCi uoml u, Hm%- N itro%gen , E leOmtheenrts ,% % %
1 6 Ch rom i u m 0 . 36-0 . 47 0 . 45-0 . 70 0 . 035 0 . 040 0 . 1 5-0 . 35 0 . 80-1 . 1 5 . . . 0 . 50-0 . 65 . . . . . . . . . Vanad i u m ,
Molyb- 0 . 25-0 . 35
den u m Al u m i n u m B
Vanad i u m 0 . 0 1 5
A The i ntentional add ition of B i , Se , Te , and Pb is not pe rm itted except fo r G rades 6 F, 8 F, and 8 FA, i n wh ich Se is specified and req u i red .
B Total al u m i n u m , sol u b l e and i nsol u b l e .
C M axi m u m , u n l ess m i n i m u m o r range is i nd icated .
D Whe re e l l i pses ({) appear i n th is tabl e the re is no req u i rement and the e l ement need not be dete rm i ned o r repo rted .
E Because of the deg ree to wh ich su lfu r seg regates , p rod uct analysis fo r su lfu r ove r 0 . 060 % max is not tech nolog ical ly app rop riate .
F As descri bed i n Specification A276/A276M .
GG rade 4 is expected to be withd rawn with i n app roxi mately 2 years . G rade 7 is an acceptable su bstitute fo r G rade 4 . See 7 . 2 .
H Col u m bi u m (Cb) and N iobi u m ( N b) are alte rnate names fo r e l ement 4 1 i n the Pe riod ic Tabl e of the E l ements .

A194/A194M - 16a

TABLE 2 Hardness Requirements A
Grade and Type Completed Nuts Sample Nut after Treatment as in 8.1.5
Brinell Hardness Rockwel C Scale l Hardness B Scale Brinell Hardness, min Rockwell Hardness B Scale, min
1 121 min ... 70 min 121 70
2 159 to 352 ... 84 min 159 84
2H to 11⁄2 in. or M36, incl 248 to 327 24 to 35 ... 179 89
2H over 11⁄2 in. or M36 212 to 327 35 max 95 min 147 79
2HM and 7M 159 to 235 ... 84 to 99 159 84
3, 4, 7, and 16 248 to 327 24 to 35 ... 201 94
6 and 6F 228 to 271 20 to 28 ... ... ...
8, 8C, 8CLN, 8M, 8T, 8F, 8P, 126 to 300 32 max 60 min ... ...
8N,
8MN, 8LN, 8MLN,
8MLCuN, 8ML4CuN,
and 9C
8A, 8CA, 8CLNA, 8MA, 8TA, 126 to 192 ... 60 to 90 ... ...
8FA, 8PA, 8NA, 8MNA,
8LNA, 8MLNA,
8MLCuNA,
8ML4CuNA,
and 9CA
8R, 8RA, 8S, and 8SA 183 to 271 25 max 88 min ... ...
A Where ellipses ({) appear in this table there is no requirement.

hot-rolled, or cold-drawn bars and shall be heat treated to meet the required mechanical properties. These grades shall be uniformly reheated to the proper austenitizing temperature (a group thus reheated being known as a quenching charge) and quenched under substantially uniform conditions for each quenching charge and tempered as shown below. Grades 2H, 2HM, 3, 4, 7, and 7M shall be liquid quenched. Grades 6 and 6F shall be quenched in liquid or inert gas. Grade 16 shall be heated to a temperature range from 1700 to 1750 °F (925 to 955 °C) and oil quenched.

Minimum Tempering Temperature, °F
Grade [°C]
2H 850 [455]
2HM 1150 [620]
3 1050 [565]
4 1100 [595]
6 and 6F 1100 [595]
7 1100 [595]
7M 1150 [620]
16 1200 [650]

Nuts machined from bar heat treated in accordance with this specification need not be reheat-treated. For Grade 2HM and 7M nuts, a final stress relief shall be done at or above the minimum tempering temperature after all forming, machining, and tapping operations. This final stress relief may be the tempering operation.

6.4.1 Grade 6 and 6F nuts shall be tempered for a minimum of 1 h at the temperature.

6.5 Grades 8, 8C, 8CLN, 8M, 8T, 8F, 8P, 8N, 8MN, 8R, 8S, 8LN, 8MLN, 8MLCuN, 8ML4CuN, and 9C nuts shall be hot or cold forged, or shall be machined from hot-forged, hotrolled or cold-drawn bars.

6.6 Grades 8A, 8CA, 8CLNA, 8MA, 8TA, 8FA, 8PA, 8NA, 8MNA, 8RA, 8SA, 8LNA, 8MLNA, 8MLCuNA, 8ML4CuNA, and 9CA nuts shall be hot- or cold-forged or shall be machined from hot-forged, hot-rolled, or cold-drawn bars and the nuts shall subsequently be carbide-solution treated by heating them for a sufficient time at a temperature to dissolve

chromium carbides followed by cooling at a rate sufficient to prevent reprecipitation of the carbides.

7 Chemical Composition

7.1 Each alloy shall conform to the chemical composition requirements prescribed in Table 1.

7.2 Grade 7 may be substituted for Grade 4. When such substitution is made, the nuts shall be marked as Grade 7.

8 Mechanical Requirements

8.1 Hardness Test:

8.1.1 Requirements:

8.1.1.1 All nuts shall meet the hardness requirements specified in Table 2.

8.1.1.2 Sample nuts of Grades 1, 2, 2H, 2HM, 3, 4, 7, 7M, and 16 which have been given the treatment described in 8.1.5 shall meet the minimum hardness specified in Table 2.

8.1.2 Number of Tests—(Grades 1, 2, 2H, 3, 4, 7, and 16 and all types of Grade 6):

8.1.2.1 Tests on the number of sample nuts in accordance with the following table shall be performed by the manufacturer following all production heat treatments:

Lot Size Samples
Up to 800 1
801 to 8000 2
8001 to 22 000 3
Over 22 000 5

8.1.2.2 In addition, a hardness test shall be performed by the manufacturer in accordance with 8.1.5 on one sample nut selected from each nominal diameter and series from each grade and heat number following completion of all production heat treatments.

8.1.3 Number of Tests, Grades 2HM and 7M:

8.1.3.1 Each nut shall be tested in accordance with either Specification A962/A962M or with Test Methods F606/F606M to ensure product conformance. The use of 100 % electromagnetic testing for hardness as an alternative to 100 % indentation

TABLE 3 Proof Load Using Threaded Mandrel — Inch Series NOTE 1—Proof loads are not design loads.
Nominal Size, in. Threads per Inch Stress Area in.2 Proof Load, IbfA
Grade 1 Grades 2, 2HM, 6, 6F, 7M Grades 2H, 3, 4, 7, 16
Heavy HexB HexC Heavy HexD HexE Heavy HexF HexG
1/4 20 0.0316 4 130 3 820 4 770 4 300 5 570 4 770
5/16 18 0.0524 6 810 6 290 7 860 7 070 9 170 7 860
3/8 16 0.0774 10 080 9 300 11 620 10 460 13 560 11 620
7/16 14 0.1063 13 820 12 760 15 940 14 350 18 600 15 940
1/2 13 0.1419 18 450 17 030 21 280 19 160 24 830 21 280
9/16 12 0.182 23 660 21 840 27 300 24 570 31 850 27 300
5/8 11 0.226 29 380 27 120 33 900 30 510 39 550 33 900
3/4 10 0.334 43 420 40 080 50 100 45 090 58 450 50 100
7/8 9 0.462 60 060 55 440 69 300 62 370 80 850 69 300
1 8 0.606 78 780 72 720 90 900 81 810 106 000 90 900
11/8 8 0.790 102 700 94 800 118 500 106 700 138 200 118 500
11/4 8 1.000 130 000 120 000 150 000 135 000 175 000 150 000
13/8 8 1.233 160 200 148 000 185 000 166 500 215 800 185 000
11/2 8 1.492 194 000 170 040 223 800 201 400 261 100 223 800
All Types of Grade 8, Grades 9C and 9CA
Heavy HexH HexI
1/4 20 0.0316 2 540 2 380
5/16 18 0.0524 4 190 3 930
3/8 16 0.0774 6 200 5 810
7/16 14 0.1063 8 500 7 970
1/2 13 0.1419 11 350 10 640
9/16 12 0.182 14 560 13 650
5/8 11 0.226 18 080 16 950
3/4 10 0.334 26 720 25 050
7/8 9 0.462 36 960 34 650
1 8 0.606 48 480 45 450
11/8 8 0.790 63 200 59 250
11/4 8 1.000 80 000 75 000
13/8 8 1.233 98 640 92 450
11/2 8 1.492 119 360 111 900
A See limit for proof load test in 8.2.2.1. The proof load for jam nuts shall be 46 % of the tabulated load.
B Based on proof stress of 130 000 psi.
C Based on proof stress of 120 000 psi.
D Based on proof stress of 150 000 psi.
E Based on proof stress of 135 000 psi.
F Based on proof stress of 175 000 psi.
G Based on proof stress of 150 000 psi.
H Based on proof stress of 80 000 psi.
I Based on proof stress of 75 000 psi.

hardness testing is permissible when qualified by sampling using indentation hardness testing. Each lot tested for hardness electromagnetically shall be 100 % examined in accordance with Practice E566. Following electromagnetic testing for hardness, a random sample of a minimum of 100 pieces in each purchase lot (as defined in 3.1.3) shall be tested by indentation hardness methods. All samples must meet hardness requirements to permit acceptance of the lot. If any one sample is outside of the specified maximum or minimum hardness, the lot shall be rejected and either reprocessed and resampled, or tested 100 % by indentation hardness methods.

8.1.3.2 In addition, 8.1.2.2 shall be met.

8.1.4 Number of Tests, All Types of Grade 8—Tests on the number of sample nuts in accordance with 8.1.2.1 shall be performed by the manufacturer.

8.1.5 Test 2—In addition to the testing required by 8.1.2.1 the manufacturer shall also perform hardness tests on sample nuts after the following test heat treatment. After completion of

all production heat treatments heat the specimen nuts to the temperatures indicated below for 24 h, then slow cool. Test at room temperature.

GradeA Temperature, °F [°C]
1 850 [455]
2, 2H, 2HM 1000 [540]
3, 7, 7M 1100 [590]
16 1200 [650]
A Nuts intended to be coated with zinc or cadmium (marked in accordance with the requirements of Supplementary Requirement S8) are not subjected to the requirements of 8.1.5 (See Appendix X2).

8.1.5.1 Special Requirement, Grades 2HM and 7M— Preparation of Grades 2HM and 7M nuts for hardness test and the hardness test itself shall be performed with consideration to (1) protect legibility of markings; (2) minimize exterior dimensional changes; and (3) maintain thread fit.

TABLE 4 Proof Load Using Threaded Mandrel — Metric NOTE 1—Proof loads are not design loads.
Nominal Size, mm Threads Pitch Stress Area mm2 Proof Load, kNA
Grade 1 Grades 2, 2HM, 6, 6F, 7M Grades 2H, 3, 4, 7, 16
Heavy HexB HexC Heavy HexD HexE Heavy HexF HexG
M6 1.0 20.1 18.0 16.6 20.8 18.7 29.2 20.8
M8 1.25 36.6 32.8 30.2 37.9 34.0 44.1 37.9
M10 1.50 58.0 51.9 47.9 60.0 53.9 69.9 60.0
M12 1.75 84.3 75.5 69.5 87.3 78.4 101.6 87.3
M14 2.0 115.0 102.9 94.9 119.0 107.0 138.6 119.0
M16 2.0 157.0 140.5 129.5 162.5 146.0 189.2 162.5
M20 2.5 245.0 219.3 202.1 253.6 227.8 295.2 253.6
M22 2.5 303.0 271.2 249.9 313.6 281.8 365.1 313.6
M24 3.0 353.0 315.9 291.2 365.4 328.3 425.4 365.4
M27 3.0 459.0 411.0 378.7 475.1 426.9 553.4 475.1
M30 3.5 561.0 502.1 462.8 580.6 521.7 676.0 580.6
M36 4.0 817.0 731.2 674.0 845.6 759.8 984.5 845.6
Nominal Size, mm All Types of Grade 8, and Grades 9C and 9CA HexI
Stress Area, mm2 Heavy HexH
M6 1.0 20.1 11.1 10.4
M8 1.25 36.6 20.1 18.8
M10 1.50 58.0 31.9 29.9
M12 1.75 84.3 46.4 43.4
M14 2.0 115.0 63.3 59.2
M16 2.0 157.0 86.4 80.9
M20 2.5 245.0 134.8 126.2
M22 2.5 303.0 166.7 156.0
M24 3.0 353.0 194.2 181.8
M27 3.0 459.0 252.5 236.4
M30 3.5 561.0 308.6 288.9
M36 4.0 817.0 449.4 420.8
A See limit for proof load test in 8.2.2.1. The proof load for jam nuts shall be 46 % of the tabulated load.
B Based on proof stress of 895 MPa.
C Based on proof stress of 825 MPa.
D Based on proof stress of 1035 MPa.
E Based on proof stress of 930 MPa.
F Based on proof stress of 1205 MPa.
G Based on proof stress of 1035 MPa.
H Based on proof stress of 550 MPa.
I Based on proof stress of 515 MPa.

8.2 Proof Load Test:

8.2.1 Requirements—The nuts listed in Tables 3 and 4 shall be capable of withstanding the proof loads specified therein. Proof load testing of nuts manufactured to dimensions and configurations other than those covered in Table 3 or Table 4 is only required when S9 is specified in the order or inquiry otherwise the nuts shall be cross-sectional hardness tested per Annex A3 of Test Methods and Definitions A370. Nuts that would require a proof load in excess of 160 000 lbf or 705 kN shall, unless Supplementary Requirements S1 or S4 are invoked in the purchase order or contract, be proof load tested per Section 8, or cross sectional hardness tested per Annex A3 of Test Methods and Definitions A370.

8.2.2 Number of Tests:

8.2.2.1 The manufacturer shall test the number of nuts specified in 8.1.2.1 following all production heat treatments. Proof Load tests prevail over hardness tests in the event a conflict exists relative to minimum strength.

8.2.3 Test Method—The test shall be run using a threaded mandrel or a test bolt in accordance with Specification A962/ A962M.

8.3 Cone Proof Load Test:

8.3.1 Requirements—This test shall be performed only when visible surface discontinuities become a matter of issue between the manufacturer and the purchaser. Nuts in the size range 1⁄4 to 1
1
⁄2 in. inclusive and M6 to M36 inclusive shall be proof load tested. Nuts not in this size range and all types of Grade 8 nuts are not subject to this test. Also, nuts manufactured to dimensions and configurations other than those covered by Specification A962/A962M, ASME B 1.1, ASME B 1.13M, ASME B 18.2.2, ASME B 18.2.4.6M, and ISO 4033 are not subject to the cone proof load test. The cone proof load applied shall be determined in accordance with the Cone Proof Load requirements in Specification A962/A962M (tables or formulae or both) based upon the proof stresses shown in Table 5 and Table 6 of Specification A194/A194M.

8.3.2 Number of Tests—The manufacturer shall sample and test the number of nuts specified in 8.1.2.1. The lot shall be considered acceptable if the sample nut(s) withstand(s) application of the cone proof load without failure.

9 Dimensions

9.1 Nuts shall be hexagonal in shape, and in accordance with the dimensions for the hex or heavy hex series, as

TABLE 5 Proof Stress Using 120° Hardened Steel Cone — Inch
Proof Stress – psi, Minimum
Type Grade 1 Grades 2, 2HM, 6, 6F & 7M Grades 2H 3, 4, 7, & 16
Hex 120 000 135 000 150 000
Heavy Hex 130 000 150 000 175 000
TABLE 6 Proof Stress Using 120° Hardened Steel Cone — Metric
Proof Stress - MPa, Minimum
Type Grade 1 Grades 2, Grades 2H
2HM, 6, 3, 4, 7, & 16
6F & 7M
Hex 825 930 1035
Heavy Hex 895 1035 1205

required, by ASME B 18.2.2, ASME B 18.2.4.6M, and ISO 4033. Unless otherwise specified, the American National Standard Heavy Hex Series shall be used and nuts shall be either double chamfered or have a machined or forged washer face, at the option of the manufacturer, and, conform to the angularity requirements of ASME B 18.2.2, ASME B 18.2.4.6M, and ISO 4033.

9.2 Unless otherwise specified, threads shall be in accordance with ASME B 1.1 or ASME B 1.13M, and shall be gauged in accordance with ASME B 1.2 and ASME B 1.13M as described in 9.2.1 and 9.2.2.

9.2.1 Nuts up to and including 1 in. nominal size shall be UNC Series Class 2B fit. Metric nuts up to and including M24 nominal size shall be coarse thread series tolerance 6H.

9.2.2 Nuts over 1 in. nominal size shall be either UNC Series Class 2B fit or 8 UN Series Class 2B fit. Unless otherwise specified, the 8 UN series shall be furnished. Metric nuts over M24 nominal size shall be coarse thread series tolerance 6H. NOTE 1—Modification of thread dimensions may result in loss of load carrying ability.

10 Workmanship, Finish, and Appearance

10.1 Nuts shall be free of defects and shall be good commercial finish.

10.2 If visible surface imperfections in size 1
⁄4 through 1
1
⁄2 in. and M6 through M36 and in any grade other than Grade 8 become a matter of issue between the manufacturer and the purchaser, the cone proof load test described in 8.3 shall be employed.

10.3 If a scale-free bright finish is required, this shall be specified on the purchase order.

11 Retests

11.1 Provisions for retests by the purchaser and his representative are specified in Supplementary Requirement S2.

12 Certification

12.1 In addition to the requirements of Specification A962/ A962M, the certification shall include the results of the chemical analysis, macroetch examination (Carbon and Alloy

Steels Only), mechanical tests, and the minimum tempering temperature for nuts of Grades 2H, 2HM, 3, 4, 6, 6F, 7, and 7M.

13 Product Marking

13.1 In addition to the requirements of Specification A962/ A962M, nuts shall be legibly marked on one face with marking representing the grade, type, and applicable manufacturing process shown in Table 7. Marking of wrench flats or bearing

TABLE 7 Marking of Nuts A
Nuts Hot- Nuts Machined Nuts Manu-
Grade and Forged or from Bar factured in
Type Cold-Punched Stock Accordance with 6.6
1 1 1B ...
2 2 2B ...
2HB 2H 2HB ...
2HMB,C 2HM 2HMB ...
3 3 3B ...
4 4 4B ...
4LD 4L 4BL ...
6 6 6B ...
6F 6F 6FB ...
7 7 7B ...
7LD 7L 7BL ...
7MB,C 7M 7MB ...
7MLB,D 7ML 7MLB
8 8 8B 8A
8C 8C 8CB 8CA
8CLN 8CLN 8CLNB 8CLNA
8M 8M 8MB 8MA
8T 8T 8TB 8TA
8F 8F 8FB 8FA
8P 8P 8PB 8PA
8N 8N 8NB 8NA
8MN 8MN 8MNB 8MNA
8R 8R 8RB 8RA
8S 8S 8SB 8SA
8LN 8LN 8LNB 8LNA
8MLN 8MLN 8MLNB 8MLNA
8MLCuN 8MLCuN 8MLCuNB 8MLCuNA
8ML4CuN 8ML4CuN 8ML4CuNB 8ML4CuNA
9C 9C 9CB 9CA
16 16 16B
A Where ellipses ({) appear in this table there is no requirement.
B The letters H and M indicate heat-treated nuts (see Section 6).
C An underline as a marking requirement for grades 2HM and 7M has been removed but is permitted.
D See Supplementary Requirement S3.

surfaces is not permitted unless agreed upon between manufacturer and purchaser.

14 Keywords

14.1 bolting; chemical analysis; coated; marking on bolting components; nuts; plated

SUPPLEMENTARY REQUIREMENTS

One or more of the following supplementary requirements shall be applied only when specified by the purchaser in the inquiry, contract, or order. Details of these supplementary requirements shall be agreed upon in writing by the manufacturer and purchaser. Supplementary requirements shall in no way negate any requirement of the specification itself.

S1. Strain-Hardened Austenitic Steel Nuts

S1.1 Strain hardened Grades 8, 8C, 8T, 8M, 8F, 8P, 8N, or 8MN nuts may be specified. When Supplementary Requirement S1 is invoked in the order, nuts shall be machined from cold drawn bars or shall be cold forged to shape. No subsequent heat treatment shall be performed on the nuts. Nuts made in accordance with this requirement shall be proof load tested in accordance with 8.2.2.1 and shall withstand the proof load specified in Table S1.1 and Table S1.2. Testing nuts requiring proof loads over 160 000 lbf or 705 kN is only required when Supplementary Requirement S4 is invoked. The hardness limits of Table 2 do not apply to strain hardened nuts. Nuts made in accordance with this requirement shall be marked with the Grade symbol underlined.

S2. Retests by Purchaser’s Representative

S2.1 The purchaser’s representative may select two nuts per keg (200-lb unit [90-kg]) for sizes 5⁄8 in. and M16 and smaller, one nut per keg for sizes over 5⁄8 in. and M16 up to and

including 1
1
⁄2 in. and M36, and one nut per every two kegs for sizes larger than 1
1
⁄2 in. and M36, which shall be subjected to the tests specified in Section 8.

S3. Low-Temperature Requirements for Grade 4, Grade 7 or Grade 7M Nuts

S3.1 When low-temperature requirements are specified for Grade 4 or Grade 7 nuts, the Charpy test procedures and requirements as defined in Specification A320/A320M for Grade L7 shall apply. When low-temperature requirements are specified for Grade 7M nuts, the Charpy test procedures and requirements as defined in Specification A320/A320M for Grade L7M shall apply. Charpy specimens may be taken from a sample nut, nut blank, or may be taken from separate test samples of the same heat processed through heat treatment with the nuts for which the test is to apply. Impact testing is not required when the bar stock or nut is smaller than 5⁄8 in. [16 mm] in diameter.

TABLE S1.1 Proof Load Testing of Strain Hardened Nuts Using Threaded Mandrel — Inch Series NOTE 1—Proof loads are not design loads.
Proof Load, lbfA
Nominal Size, in. Threads per in. Stress Area, in.2 Grade 8M (strain hardened) Grade 8M (strain hardened) All Other Types of Grade 8 (strain hardened) All Other Types of Grade 8 (strain hardened)
Heavy HexB HexC Heavy HexD HexB
1/4 20 0.0316 3 480 3 160 3 950 3 480
5/16 18 0.0523 5 760 5 240 6 550 5 760
3/8 16 0.0774 8 510 7 740 9 675 8 510
7/16 14 0.1063 11 690 10 630 13 290 11 690
1/2 13 0.1419 15 610 14 190 17 740 15 610
9/16 12 0.182 20 020 18 200 22 750 20 020
5/8 11 0.226 24 860 22 600 28 250 24 860
3/4 10 0.334 36 740 33 400 41 750 36 740
7/8 9 0.462 46 200 41 580 53 130 46 200
1 8 0.606 60 600 54 540 69 690 60 600
11/8 8 0.790 75 050 67 150 82 950 75 050
11/4 8 1.000 95 000 85 000 105 000 95 000
13/8 8 1.233 110 970 98 640 123 300 110 970
11/2 8 1.492 134 280 119 360 149 200 134 280
A The proof load for jam nuts shall be 46 % of the tabulated value.
B Based on proof stress of 110 000 psi up to 3⁄4 in.; 100 000 psi 7 ⁄8 to 1 in.; 95 000 psi 1 1 ⁄8 to 1 1 ⁄4 in.; 90 000 psi 1 3 ⁄8 to 1 1 ⁄2 in.
C Based on proof stress of 100 000 psi up to 3⁄4 in.; 90 000 psi 7 ⁄8 to 1 in.; 85 000 psi 1 1 ⁄8 to 1 1 ⁄4 in.; 80 000 psi 1 3 ⁄8 to 1 1 ⁄2 in.
D Based on proof stress of 125 000 psi up to 3⁄4 in.; 115 000 psi 7 ⁄8 to 1 in.; 105 000 psi 1 1 ⁄8 to 1 1 ⁄4 in.; 100 000 psi 1 3 ⁄8 to 1 1 ⁄2 in.
TABLE S1.2 Proof Load Testing of Strain Hardened Nuts Using Threaded Mandrel—Metric NOTE 1—Proof loads are not design loads.
Proof Load, kNA
Nominal Size, mm Thread Pitch Stress Area, mm2 Grade 8M (strain hardened) Grade 8M (strain hardened) All Other Types of Grade 8 (strain hardened) All Other Types of Grade 8 (strain hardened)
Heavy HexB HexC Heavy HexD HexB
M6 1.0 20.1 15.3 13.9 17.3 15.3
M8 1.25 36.6 27.8 25.3 31.3 27.8
M10 1.50 58.0 44.1 40.0 49.9 44.1
M12 1.75 84.3 64.1 58.2 72.5 64.1
M14 2.0 115.0 87.4 79.4 98.9 87.4
M16 2.0 157.0 119.3 108.3 135.0 119.3
M20 2.5 245.0 186.2 169.0 210.9 186.2
M22 2.5 303.0 209.0 187.9 240.9 209.0
M24 3.0 353.0 243.5 218.9 280.6 243.5
M27 3.0 459.0 300.6 268.5 332.7 300.6
M30 3.5 561.0 367.5 328.2 406.7 367.5
M36 4.0 817.0 506.5 449.4 563.7 506.5
A The proof load for jam nuts shall be 46 % of the tabulated value.
B Based on proof stress of 760 MPa up to M20 mm; 690 MPa M22 to M24 mm; 655 MPa M27 to M30; and 620 MPa for M36.
C Based on proof stress of 690 MPa up to M20 mm; 620 MPa M22 to M24 mm; 585 MPa M27 to M30; and 550 MPa for M36.
D Based on proof stress of 860 MPa up to M20 mm; 795 MPa M22 to M24 mm; 725 MPa M27 to M30 mm; and 690 MPa for M36.

S3.2 An “L” shall be added to the marking, as shown in Table 7, for nuts so tested.

S4. Proof Load Tests of Large Nuts

S4.1 Proof load testing of nuts requiring proof loads of over 160 000 lbf or 705 kN is required. Testing shall be performed in accordance with 8.2 to the loads required in Table S4.1 and Table S4.2. The maximum load will be based entirely on the equipment available.

S5. Control of Product by Heat Number

S5.1 When control of nuts by actual heat analysis is required and this supplementary requirement is specified, the manufacturer shall identify the completed nuts in each shipment by the actual heat number. When this supplementary requirement is specified, a certificate including the results of the actual production tests of each test lot together with the heat chemical analysis shall be furnished by the manufacturer.

S6. Grain Size Requirements for Non H Grade Austenitic Steels Used Above 1000 °F

S6.1 For design metal temperatures above 1000 °F [540 °C], the material shall have a grain size of No. 7 or coarser as determined in accordance with Test Methods E112. The grain size so determined shall be reported on the Certificate of Test.

S7. Coating on Nuts

S7.1 It is the purchaser’s responsibility to specify in the purchase order all information required by the coating facility. Examples of such information may include but are not limited to the following:

S7.1.1 Reference to the appropriate coating specification and type, thickness, location, modification to dimensions, and hydrogen embrittlement relief. NOTE S7.1—Modification of thread dimensions may result in loss of load carrying ability.

TABLE S4.1 Proof Load for Large Heavy Hex Nuts — Inch A
Nominal Size, in. Threads per in. Stress Area, in.2 Proof Load, lbfB
Grade 1 Heavy Hex Grades 2, 2HM, 6, 6F, 7M Heavy Hex Grades 2H, 3, 4, 7, 16 Heavy Hex
15/8 8 1.78 231 400 267 000 311 500
13/4 8 2.08 270 400 312 000 364 000
17/8 8 2.41 313 300 361 500 421 800
2 8 2.77 360 100 415 500 484 800
21/4 8 3.56 462 800 534 000 623 000
21/2 8 4.44 577 200 666 000 777 000
23/4 8 5.43 705 900 814 500 950 250
A ASME B18.2.2 in the size range over 1 1 ⁄2 in. provides dimensions only for heavy hex nuts. Refer to 8.3.1.
B Proof loads for nuts of larger dimensions or other thread series may be calculated by multiplying the thread stress area times the proof stress in the notes to Table 3 or Table S1.1. The proof load for jam nuts shall be 46 % of the tabulated load.
TABLE S4.2 Proof Load for Large Heavy Hex Nuts — Metric A
Nominal Size, mm Thread Pitch Stress Area, mm2 Proof Load, kNB
Grade 1 Heavy Hex Grades 2, 2HM, 6, 6F, 7M Heavy Hex Grades 2H, 3, 4, 7, 16 Heavy Hex
M42 4.5 1120 1002.4 1159.2 1349.6
M48 5 1470 1315.7 1521.4 1771.4
M56 5.5 2030 1816.9 2101.0 2446.2
M64 6 2680 2398.6 2773.8 3229.4
M72 6 3460 3096.7 3581.1 4169.3
A ASME B 18.2.4.6M in the size range over M36 provides dimensions only for heavy hex nuts. Refer to 7.3.1.
B Proof loads for nuts of larger dimensions or other thread series may be calculated by multiplying the thread stress area times the proof stress in the notes to Table 4 or Table S1.2. The proof load for jam nuts shall be 46 % of the tabulated load.

S7.1.2 Reference to Specifications A153/A153M, B633, B695, B696, B766, F1941/F1941M, F2329/F2329M, or Test Method F1940, or other standards.

S8. Marking Coated Nuts

S8.1 Nuts coated with zinc shall have ZN marked after the grade symbol. Nuts coated with cadmium shall have CD marked after the grade symbol. NOTE S8.1—As an example, the marking for zinc-coated 2H bolting components will now be 2HZN rather than 2H*.

S9. Proof Load Testing

S9.1 Proof load tests of nuts made to dimensions, thread pitch, and configurations other than those covered in Table 3 or Table 4 shall be made using loads agreed upon between the manufacturer and the purchaser.

S10. 100 % Hardness Testing of Grade 2HM and 7M

S10.1 Each nut shall be tested for hardness by indentation method and shall meet the requirements specified in Table 2.

APPENDIXES

(Nonmandatory Information)

X1. STRAIN HARDENING OF AUSTENITIC STEELS

X1.1 Strain hardening is the increase in strength and hardness that results from plastic deformation below the recrystallization temperature (cold work). This effect is produced in austenitic stainless steels by reducing oversized bars to the desired final size by cold drawing or other process. The degree of strain hardening achievable in any alloy is limited by its strain hardening characteristics. In addition, the amount of strain hardening that can be produced is further limited by the variables of the process, such as the total amount of cross-

section reduction, die angle and bar size. In large diameter bars, for example, plastic deformation will occur principally in the outer regions of the bar, so that the increased strength and hardness due to strain hardening is achieved predominantly near the surface of the bar. That is, the smaller the bar, the greater the penetration of strain hardening. Thus, the mechanical properties of a given strain hardened bolting component are dependent not just on the alloy, but also on the size of bar from which it is machined.

X2. COATINGS AND APPLICATION LIMITS

X2.1 Use of coated bolting components at temperatures above approximately one-half the melting point (Fahrenheit or Celsius) of the coating is not recommended unless consideration is given to the potential for liquid and solid metal embrittlement, or both. The melting point of elemental zinc is approximately 780 °F [415 °C]. Therefore, application of zinc

coated bolting components should be limited to temperatures less than 390 °F [210 °C]. The melting point of cadmium is approximately 600 °F [320 °C]. Therefore, application of cadmium coated bolting components should be limited to temperatures less than 300 °F [160 °C].

Committee A01 has identified the location of selected changes to this specification since the last issue, A194/A194M–16, that may impact the use of this specification. (Approved December 1, 2016)

(1) Added Note 1.

(2) Revised 8.2.

Committee A01 has identified the location of selected changes to this specification since the last issue, A194/A194M–15a, that may impact the use of this specification. (Approved May 1, 2016)

(1) Revised 6.3.1 and 6.3.2.

Committee A01 has identified the location of selected changes to this specification since the last issue, A194/A194M–15, that may impact the use of this specification. (Approved November 1, 2015)

(1) Changed the word “fastener” to “bolting component” in (2) Revised 13.1 and Table 7 title for clarity. accordance with the definitions of the common requirements of Specification in 5.1, 14, Supplement S8.1, and X1.1 and X2.1.

This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years and if not revised, either reapproved or withdrawn. Your comments are invited either for revision of this standard or for additional standards and should be addressed to ASTM International Headquarters. Your comments will receive careful consideration at a meeting of the responsible technical committee, which you may attend. If you feel that your comments have not received a fair hearing you should make your views known to the ASTM Committee on Standards, at the address shown below.

资源下载此资源下载价格为5金币立即购买,VIP免费

1.本站大部份文档均属免费,部份收费文档,经过本站分类整理,花了精力和时间,收费文档是为了网站运营成本等费用开支;
2.购买会员:全部免费下载本站资源(或单次下载)即视为对网站的赞助、打赏,非商业交易行为(不认同此观点请勿支付)请慎重考虑;
3.所有收费文档都真实可靠,为了节约成本,文档在网站前台不做预览,如果付费后,与实际文档不符合,都可以加微信号:pdftj888申请退款;
4.付费下载过程中,如果遇到下载问题,都可以加微信号pdftj888解决;
5.手机支付,尽量选择支付宝支付;
6.如图集或者标准不清楚,在本站找不到您需要的规范和图集,希望增加资料等任何问题,可联系微信号:pdftj888解决;

文档天下
  • 本文由 发表于 2026年11月24日 08:32:36
  • 转载请务必保留本文链接:https://www.998pdf.com/84167.html
匿名

发表评论

匿名网友 填写信息

:?: :razz: :sad: :evil: :!: :smile: :oops: :grin: :eek: :shock: :???: :cool: :lol: :mad: :twisted: :roll: :wink: :idea: :arrow: :neutral: :cry: :mrgreen: